Wear-resistant titanium alloy nano-injection polyamide composite material and preparation method thereof
By modifying additives such as metal sulfide and calcium hypophosphate, the binding force and wear resistance of titanium alloy nano-injection molded polyamide composite materials are improved, and the wear problem of titanium alloy materials in the folding screen hinge in the prior art is solved, and the wear problem of titanium alloy materials in the folding screen hinge is realized. High binding force and wear resistance.
Patent Information
- Application Number
- CN202311855303.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing nanoinjection molding materials are prone to surface wear and debris fall off after multiple openings and closings of the folding screen hinge. The nanoinjection molding properties of titanium alloys are inconsistent with aluminum alloys or stainless steels, and lack solutions that can be both high binding and wear-resistant.
Wear-resistant titanium alloy nano-injection molded polyamide composite materials using modified metal sulfide, calcium hypophosphate and maleic anhydride graft toughening agent to improve the binding force and wear resistance of titanium alloy and plastic through specific preparation methods. performance.
It realizes high binding force (>35MPa) and good wear resistance of titanium alloy nanoinjection molded materials, suitable for folding screen hinges and midframe materials, simplifying the preparation process for large-scale production.
Smart Images

Figure CN117551346B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and particularly relates to a wear-resistant titanium alloy nano-injection polyamide composite material and a preparation method and application thereof. Background Art
[0002] The nano injection molding process (NMT) invented by Taisei of Japan can directly adhere modified polyphenylene sulfide (PPS), modified butylene terephthalate (PBT) and other materials to the metal surface treated by nanotechnology through injection molding (patent text WO 2007 / 040245, etc.). Subsequent public patent texts (CN111117232A, CN202210592626.0, etc.) describe the improved NMT technology, which can be combined with metals and ceramics. NMT technology has now been rapidly popularized in the mobile phone industry. With the rapid development of folding screen mobile phones, NMT technology has been promoted and applied to the hinge structure of folding screens. In actual applications, it is found that the current NMT materials are prone to surface wear and debris shedding after multiple opening and closing of the hinge, which not only affects the appearance, but also the shedding debris will cause secondary damage to the hinge structure. Therefore, the industry has put forward higher requirements for the wear resistance of NMT plastics.
[0003] Polytetrafluoroethylene (PTFE) and molybdenum disulfide are commonly used plastic wear-resistant additives that can effectively reduce the friction coefficient and wear rate of plastics. However, a higher addition amount is required to achieve a significant effect, generally greater than 10%. At the same time, experiments have shown that the addition of high content PTFE and molybdenum disulfide will significantly reduce the NMT bonding force and the mechanical properties of the material, causing cracking of the metal-plastic bond or cracking of the plastic itself in the subsequent process. Therefore, PTFE and molybdenum disulfide are not suitable for wear-resistant NMT plastic materials.
[0004] As the demand for lightweight mobile phones continues to grow, replacing stainless steel with titanium alloy will become a new trend. The industry has found that the nano-injection molding performance of titanium alloy is not consistent with that of aluminum alloy and stainless steel. Plastic products that have high bonding strength with aluminum alloy or stainless steel often have low bonding strength with titanium alloy. At present, there is no mature solution in the industry that has both high nano-injection molding bonding strength (>35MPa) with titanium alloy and good wear resistance. Summary of the invention
[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a wear-resistant titanium alloy nano-injection-molded polyamide composite material.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned wear-resistant titanium alloy nano-injection-molded polyamide composite material.
[0007] Another object of the present invention is to provide an application of the above-mentioned wear-resistant titanium alloy nano-injection-molded polyamide composite material.
[0008] The purpose of the present invention is achieved through the following solutions:
[0009] A wear-resistant titanium alloy nano-injection polyamide composite material, comprising the following components in percentage by weight:
[0010]
[0011] The wear-resistant titanium alloy nano-injection polyamide composite material may further include at least one of an antioxidant and a release agent, wherein the weight percentage of the antioxidant is 0.05%-0.5%, and the weight percentage of the release agent is 0.1%-2.0%.
[0012] Furthermore, the weight percentage of the modified metal sulfide in the wear-resistant titanium alloy nano-injection-molded polyamide composite material is 4-6%, preferably 5%.
[0013] Furthermore, the weight percentage of the calcium hypophosphite is 0.1-0.6%, preferably 0.3%-0.6%.
[0014] Furthermore, the toughening agent is a maleic anhydride grafted toughening agent, more preferably maleic anhydride ethylene octene copolymer, with a weight percentage of 3%-6%.
[0015] Furthermore, the glass fiber is cylindrical glass fiber or flat glass fiber.
[0016] Furthermore, the antioxidant is antioxidant 1098.
[0017] Furthermore, the release agent is NylostabS-EED.
[0018] The above-mentioned modified metal sulfide is prepared by the following method:
[0019] (1) mixing molybdenum disulfide, bismuth sulfide and copper sulfate, evacuating the mixture, and then heating the mixture for reaction. After the reaction is completed, the mixture is naturally cooled, and the reaction product is taken out and ground into powder;
[0020] (2) mixing the reaction product ground in step (1), a monohydric alcohol, an organic amine, and a silane coupling agent, and then heating and refluxing the mixture, and cooling the mixture naturally after the reaction is completed, filtering the mixture, and then heating and aging the mixture to obtain a modified metal sulfide.
[0021] In the preparation process of the modified metal sulfide, the amounts of the five raw materials used meet the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine and silane coupling agent is 20-30:20-30:40-60:3-5:1-3.
[0022] Preferably, in the preparation process of the modified metal sulfide, the amounts of the five raw materials used satisfy the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine and silane coupling agent is 25:25:50:4:2.
[0023] The heating reaction described in step (1) refers to heating to 700-900° C. and maintaining for 12-36 hours.
[0024] The organic amine in step (2) is a small molecule polar substance, which can better adhere to the surface of the sulfide powder, and is convenient for forming hydrogen bonds with the coupling agent or reacting with the active groups of the coupling agent. The silane coupling agent modifies the reactant in step (1) to form a good interface with the plastic.
[0025] The monohydric alcohol described in step (2) refers to at least one of the monohydric alcohols with less than 6 carbon atoms, preferably ethanol, wherein the purpose of ethanol is to play a dispersing role.
[0026] The organic amine described in step (2) is at least one of triethylamine and hydrazine hydrate, preferably hydrazine hydrate.
[0027] The silane coupling agent described in step (2) is at least one of vinyl silane, amino silane, methacryloxy silane and epoxy silane, preferably γ-aminopropyltriethoxy silane.
[0028] The heating reflux time in step (2) is 10-15h.
[0029] The aging described in step (2) refers to aging at 150-180° C. for 2-6 hours.
[0030] A method for preparing the wear-resistant titanium alloy nano-injection polyamide composite material comprises the following steps: mixing the components and extruding and granulating them through an extruder, wherein the granulation temperature is 240-320°C.
[0031] The above-mentioned wear-resistant titanium alloy nano-injection-molded polyamide composite material is used in the preparation of mobile phone folding screen hinges and middle frame materials, especially in titanium alloy folding screen hinges and middle frame materials.
[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0033] (1) The polyamide composite material provided by the present invention has a very high titanium alloy nano-injection molding bonding strength, which is greater than 35 MPa.
[0034] (2) The polyamide composite material provided by the present invention has excellent wear resistance.
[0035] (3) The preparation method of the present invention is simple and easy to implement, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The schematic diagram of the structure of the titanium alloy plastic test piece is shown in FIG. 1 , titanium alloy part; and 2, plastic part.
[0037] Figure 2 This is the infrared spectrum of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours.
[0038] Figure 3 The actual pictures and scanning electron microscope pictures of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours, wherein (a) represents before calcination and (b) represents after calcination.
[0039] Figure 4 XRF elemental analysis characterization of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours, wherein (a) represents before calcination and (b) represents after calcination. DETAILED DESCRIPTION
[0040] The present invention will be described in further detail below in conjunction with examples and accompanying drawings, but the embodiments of the present invention are not limited thereto. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0041] The polyamide of the present application and its preparation method are described in detail below using examples. The preparation method of the polyamide PA106 / 10T (7:3) in the examples is as follows:
[0042] 1) Add 10 kg of deionized water into a 50 L automatic control polymerization kettle with a stirrer, then add 25 kg of a monomer mixture (wherein the molar ratio of adipic acid to terephthalic acid in the monomer mixture is 7:3, and the ratio of the total molar amount of adipic acid and terephthalic acid to the molar amount of decanediamine is 1:1), add 1 g of phosphoric acid, and carry out a dehydration reaction at a pressure of 26 bar and a temperature of 300° C. in the polymerization kettle;
[0043] 2) After the reaction, nitrogen is injected to expel the water generated by the reaction, and then the polyamide melt is discharged under pressure. The melt is formed by a die casting belt and is obtained by cooling and pelletizing.
[0044] The remaining raw materials can be obtained commercially, as follows: cylindrical glass fiber is Chongqing International ECS301HP, flat glass fiber is Chongqing International ECS301HF, maleic anhydride grafted ethylene octene copolymer is DuPont N493, antioxidant 1098 is Tianjin Lianlong 1098, SEED (release agent) is Clariant NylostabS-EED, calcium hypophosphite is purchased from Suzhou Lianxiong Chemical Co., Ltd., and diethyl aluminum hypophosphite is Clariant OP1230.
[0045] The wear resistance test in the following embodiments was conducted using the GBT3960-2016 standard method.
[0046] The titanium alloy nano-injection molding sample used in the present invention is prepared by the following process: Grade 5 titanium alloy material, size specifications, length 45mm, width 18mm, thickness 1.6mm; surface treatment process: sequentially immerse in NaOH solution alkaline washing (2mol / L, 50℃, 20 seconds), hydrochloric acid corrosion (1.5mol / L, 35℃, 40 seconds), and ammonia solution (2mol / L, 30℃, 4 minutes), and then the immersed sample is cleaned with water and dried to obtain a titanium alloy sample with nanopores on the surface.
[0047] Preparation of the plastic titanium alloy test monolith used in the present invention:
[0048] The present invention refers to the method of Japanese Dacheng nano injection molding related patent (US8057890 (B2)) to prepare the plastic metal test integral part. Figure 1 This is a schematic diagram of the structure of the titanium alloy plastic test piece. The size of the titanium alloy sheet is 18mm×45mm×1.6mm, the size of the plastic part is 10mm×45mm×3mm, and the bonding area between the plastic and the titanium alloy is 0.5cm 2 In all experiments, the injection molding maintained the same injection molding conditions, barrel temperature 260-300°C, mold temperature 150°C, and the plastic compound was injected onto the titanium alloy sheet to obtain a plastic titanium alloy test piece.
[0049] Plastic-metal bonding performance test:
[0050] The metal-plastic bonding strength test standard used in the present invention refers to the standard in the Japanese Daisei Chemical patent (US8057890 (B2)), and the plastic-metal bonding area is 0.5 cm 2 , a biaxial tensile test is performed on the test piece.
[0051] The preparation process of the plastic composite material is as follows: weigh the components in corresponding amounts according to weight percentage, then mix the components, and granulate the plastic composite using a twin-screw extruder at a granulation temperature of 240 to 320°C.
[0052] Example 1
[0053] Mix 100g of molybdenum disulfide, 400g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product A.
[0054] Example 2
[0055] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B.
[0056] The infrared spectra of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate before and after calcination at 800℃ for 24h are as follows Figure 2 As shown, the peak of SO4 at position 1197 disappears, indicating that the decomposition of copper sulfate at high temperature produces CuO and SO3; after high-temperature calcination, there is an obvious absorption peak at position 1080, indicating that metal persulfate components are generated. The high-temperature reaction process includes chemical reaction + physical doping process.
[0057] During the high temperature reaction, the mixture undergoes an obvious phase change. After calcination, the powdery white substance is not found when the image is magnified 1000 times, indicating that the copper sulfate is almost completely decomposed and copper oxide is generated at high temperature. Copper oxide and sulfide are physically doped, generating sulfide-doped copper oxide.
[0058] Example 2A
[0059] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of triethylamine, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B1.
[0060] Example 2B
[0061] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 20g of hydrazine hydrate, 40g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B2.
[0062] Example 3
[0063] Mix 400g of molybdenum disulfide, 100g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product C.
[0064] Example 4
[0065] Mix 400g of molybdenum disulfide, 400g of bismuth sulfide and 200g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product D.
[0066] Example 5
[0067] This example aims to study the effects of different modified metal sulfides on the titanium alloy bonding and wear resistance of the polyamide composite.
[0068] PA106 / 10T resin, modified metal sulfide and other additives were mixed according to the weight percentages shown in Table 1, and extruded into granules by a twin-screw extruder at a granulation temperature of 240-320° C. The corresponding properties of the obtained PA106 / 10T composite are shown in Table 1.
[0069] Table 1 Component weight percentage and performance data of PA106 / 10T composite
[0070]
[0071] From the data in Table 1, it can be seen that when conventional wear-resistant additives PTFE or molybdenum disulfide are added, the bonding strength of titanium alloy NMT drops sharply. However, when suitable modified metal sulfide additives are added, the bonding strength of titanium alloy NMT of the material can be well maintained, and at the same time, the wear resistance is also greatly improved, especially in Test Example 6, which can obtain the best comprehensive performance.
[0072] Example 6
[0073] This example aims to study the effect of calcium hypophosphite on the titanium alloy bonding and wear resistance of the polyamide composite.
[0074] PA106 / 10T resin, calcium hypophosphite and other additives were mixed according to the weight percentages shown in Table 2, and extruded into granules by a twin-screw extruder at a granulation temperature of 240-320° C. The corresponding properties of the obtained PA106 / 10T composite are shown in Table 2.
[0075] Table 2 Component weight percentage and performance data of PA106 / 10T composite
[0076]
[0077]
[0078] From the data in Table 2, it can be seen that although Test Example 6 has good wear resistance and high titanium alloy NMT bonding strength, its titanium alloy NMT bonding strength is still insufficient. The industry usually requires NMT bonding strength to reach 35MPa or more to achieve a high scale production success rate. When a certain amount of calcium hypophosphite is added to the system, the titanium alloy bonding strength can be greatly improved to meet the industry standard.
[0079] It can be seen from Test Examples 6 and 11-16 that with the increase in the amount of calcium hypophosphite used, the titanium alloy bonding strength increases and then decreases, and the mass wear first decreases and then increases. That is, when the weight percentage of calcium hypophosphite is 0.3-0.6%, better titanium alloy bonding strength and mass wear can be achieved at the same time.
[0080] From the comparison between Test Example 12 and Test Example 13, it can be seen that when flat glass fibers are used, the resulting composite material has higher wear resistance and higher bonding strength to titanium alloy than cylindrical glass fibers.
[0081] From the comparison between Test Examples 12, 15 and 17-18, it can be seen that when diethylaluminum hypophosphite, an analog of calcium hypophosphite, is used, a similar effect cannot be achieved.
[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A wear-resistant titanium alloy nano-injection polyamide composite material, Features The composition comprises the following components in weight percentage: Polyamide 40%-80%; Modified metal sulfide 1%-10%; Calcium hypophosphite 0.3%-6%; Toughening agent 1%-10%; Glass fiber 10%-50%; The modified metal sulfide is prepared by the following method: (1) Molybdenum disulfide, bismuth sulfide and copper sulfate are mixed, vacuumized, and then heated for reaction. After the reaction is completed, the mixture is naturally cooled, and the reaction product is taken out and ground into powder; (2) mixing the reaction product after grinding in step (1), a monohydric alcohol, an organic amine, and a silane coupling agent, and then heating to reflux for reaction. After the reaction is completed, the mixture is naturally cooled, filtered, and then heated and aged to obtain a modified metal sulfide; In the preparation process of the modified metal sulfide, the amounts of the five raw materials used meet the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine and silane coupling agent is 20-30:20-30:40-60:3-5:1-3; The heating reaction in step (1) refers to heating to 700-900°C and maintaining for 12-36 hours; The heating reflux time in step (2) is 10-15h; The aging described in step (2) refers to aging at 150-180° C. for 2-6 hours.
2. The wear-resistant titanium alloy nano-injection-molded polyamide composite material according to claim 1, Features: The weight percentage of the modified metal sulfide in the wear-resistant titanium alloy nano-injection-molded polyamide composite material is 4-6%.
3. The wear-resistant titanium alloy nano-injection-molded polyamide composite material according to claim 1, Features: The toughening agent is a maleic anhydride grafted toughening agent; The glass fiber is cylindrical glass fiber or flat glass fiber.
4. The wear-resistant titanium alloy nano-injection-molded polyamide composite material according to claim 1, Features: The wear-resistant titanium alloy nano-injection-molded polyamide composite material further comprises at least one of an antioxidant and a release agent, wherein the weight percentage of the antioxidant is 0.05%-0.5%, and the weight percentage of the release agent is 0.1%-2.0%.
5. The wear-resistant titanium alloy nano-injection-molded polyamide composite material according to claim 1, Features: The monohydric alcohol described in step (2) refers to at least one of the monohydric alcohols with less than 6 carbon atoms; The organic amine in step (2) is at least one of triethylamine and hydrazine hydrate; The silane coupling agent described in step (2) is at least one of vinyl silane, amino silane, methacryloxy silane and epoxy silane.
6. The method for preparing the wear-resistant titanium alloy nano-injection-molded polyamide composite material according to any one of claims 1 to 5, Features The method comprises the following steps: mixing the components and extruding and granulating the mixture through an extruder, wherein the granulation temperature is 240-320°C.
7. Use of the wear-resistant titanium alloy nano-injection-molded polyamide composite material according to any one of claims 1 to 5 in the preparation of mobile phone folding screen hinges and middle frame materials.
Citation Information
Patent Citations
Composite of aluminum alloy and resin and manufacturing method thereof
US8057890B2
Composite of metal with resin and process for producing the same
WO2007040245A1
Method of preparing composite material for handles
CN109679333A
Polyamide-based sliding material
CN109983105A