Wear-resistant titanium alloy nano-injection polyester composite material and preparation method thereof

By combining modified metal sulfides with titanium alloy, polyester resin and other components, wear-resistant titanium alloy nanoinjection molded polyester composite materials are prepared, which solves the poor performance and insufficient wear resistance of titanium alloy nanoinjection molding in the prior art. The problem of this is to achieve high bonding force and wear resistance, and is suitable for folding screen hinge materials.

CN118109024BActive Publication Date: 2024-11-29GUANGZHOU CNDONG NEW MATERIALS CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311855313.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-29
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Existing nanoinjection molding materials are prone to surface wear and debris fall off after multiple openings and closings of the folding screen hinge. The nanoinjection molding performance of titanium alloy is inconsistent with aluminum alloy or stainless steel, and lacks solutions that can be both high binding and wear-resistant. .

Method used

Modified metal sulfides are used as additives to prepare modified metal sulfides through specific synthetic methods, and mixed with components such as titanium alloys, polyester resins, PETs, antioxidants, mold release agents, toughening agents, etc., and then extrude The machine is used to prepare wear-resistant titanium alloy nano-injection molded polyester composite material for folding screen hinges and midframe materials.

Benefits of technology

The titanium alloy nanoinjection molding binding force is greater than 35MPa and good wear resistance, which is suitable for large-scale production, and shows high binding force and wear resistance in the titanium alloy folding screen hinge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118109024B_ABST
    Figure CN118109024B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of composite materials, and discloses a wear-resistant titanium alloy nano-injection polyester composite material and its preparation method and application. The composite material comprises the following components in weight percentage: PBT 25%-60%; PET 10-30%; modified metal sulfide 1%-10%; diethyl zinc hypophosphite 0.1%-0.8%; toughening agent 1%-10%; glass fiber 10%-50%. The modified metal sulfide is prepared by the following method: molybdenum disulfide, bismuth sulfide and copper sulfate are mixed, added into a reaction tube for vacuum heating reaction, cooled, the reaction product is taken out and ground into powder, and then mixed with monohydric alcohol, organic amine, silane coupling agent, and then heated for reflux reaction, cooled, filtered, and then heated for aging to obtain the modified metal sulfide. The polyester composite material provided by the present invention has a very high titanium alloy nano-injection bonding force, and the bonding force is greater than 35MPa. And it has good wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and particularly relates to a wear-resistant titanium alloy nano-injection polyester composite material and a preparation method and application thereof. Background Art

[0002] The nano injection molding process (NMT) invented by Taisei of Japan can directly adhere modified polyphenylene sulfide (PPS), modified butylene terephthalate (PBT) and other materials to the metal surface treated by nanotechnology through injection molding (patent WO 2007 / 040245, etc.). Subsequent patent disclosures (CN111117232A, CN202210592626.0, etc.) describe the improved NMT technology, which can be combined with metals and ceramics. NMT technology has now been rapidly popularized in the mobile phone industry. With the rapid development of folding screen mobile phones, NMT technology has been promoted and applied to folding screen hinge structures. In actual applications, it is found that the current NMT materials are prone to surface wear and debris shedding after multiple opening and closing of the hinge, which not only affects the appearance, but also the shedding debris will cause secondary damage to the hinge structure. Therefore, the industry has put forward higher requirements for the wear resistance of NMT plastics.

[0003] Polytetrafluoroethylene (PTFE) and molybdenum disulfide are commonly used plastic wear-resistant additives that can effectively reduce the friction coefficient and wear rate of plastics. However, a higher addition amount is required to achieve a significant effect, generally greater than 10%. At the same time, experiments have shown that the addition of high content PTFE and molybdenum disulfide will significantly reduce the NMT bonding force and the mechanical properties of the material, causing cracking of the metal-plastic bond or cracking of the plastic itself in the subsequent process. Therefore, PTFE and molybdenum disulfide are not suitable for wear-resistant NMT plastic materials.

[0004] As the demand for lightweight mobile phones continues to grow, replacing stainless steel with titanium alloy will become a new trend. The industry has found that the nano-injection molding performance of titanium alloy is not consistent with that of aluminum alloy and stainless steel. Plastic products that have high bonding strength with aluminum alloy or stainless steel often have low bonding strength with titanium alloy. At present, there is no mature solution in the industry that has both high nano-injection molding bonding strength (>35MPa) with titanium alloy and good wear resistance. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a wear-resistant titanium alloy nano-injection polyester composite material.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned wear-resistant titanium alloy nano-injection-molded polyester composite material.

[0007] Another object of the present invention is to provide an application of the above-mentioned wear-resistant titanium alloy nano-injection-molded polyester composite material.

[0008] The purpose of the present invention is achieved through the following solutions:

[0009] A wear-resistant titanium alloy nano-injection polyester composite material, comprising the following components in percentage by weight:

[0010]

[0011] Furthermore, the wear-resistant titanium alloy nano-injection polyester composite material may further include at least one of an antioxidant and a release agent, wherein the weight percentage of the antioxidant is 0.05%-0.5%, and the weight percentage of the release agent is 0.1%-2.0%.

[0012] Furthermore, the weight percentage of PET in the wear-resistant titanium alloy nano-injection-molded polyester composite material is 15%-25%.

[0013] Furthermore, the weight percentage of diethyl zinc hypophosphite in the wear-resistant titanium alloy nano-injection polyester composite material is 0.2%-0.5%.

[0014] Furthermore, in the wear-resistant titanium alloy nano-injection polyester composite material, the toughening agent is a copolymerized glycidyl ether toughening agent, preferably ethylene methyl methacrylate glycidyl ether copolymer, with a weight percentage of 4%-8%.

[0015] Furthermore, the weight percentage of the modified metal sulfide in the wear-resistant titanium alloy nano-injection polyester composite material is 4-6%.

[0016] Furthermore, the glass fiber is cylindrical glass fiber or flat glass fiber, preferably flat glass fiber.

[0017] Furthermore, the antioxidant is antioxidant 1010.

[0018] Furthermore, the release agent is pentaerythritol tetrastearate.

[0019] Furthermore, the modified metal sulfide is prepared by the following method:

[0020] (1) mixing molybdenum disulfide, bismuth sulfide and copper sulfate, evacuating the mixture, and then heating the mixture for reaction. After the reaction is completed, the mixture is naturally cooled, and the reaction product is taken out and ground into powder;

[0021] (2) mixing the reaction product ground in step (1), a monohydric alcohol, an organic amine, and a silane coupling agent, and then heating and refluxing the mixture, and cooling the mixture naturally after the reaction is completed, filtering the mixture, and then heating and aging the mixture to obtain a modified metal sulfide.

[0022] In the preparation process of the modified metal sulfide, the amounts of the five raw materials used meet the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine and silane coupling agent is 20-30:20-30:40-60:3-5:1-3.

[0023] Preferably, in the preparation process of the modified metal sulfide, the amounts of the five raw materials used satisfy the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine, and silane coupling agent is 25:25:50:4:2.

[0024] The heating reaction described in step (1) refers to heating to 700-900° C. and maintaining for 12-36 hours.

[0025] The organic amine in step (2) is a small molecule polar substance, which can better adhere to the surface of the sulfide powder, and is convenient for forming hydrogen bonds with the coupling agent or reacting with the active groups of the coupling agent. The silane coupling agent modifies the reactant in step (1) to form a good interface with the plastic.

[0026] The monohydric alcohol described in step (2) refers to at least one of the monohydric alcohols with less than 6 carbon atoms, preferably ethanol, wherein the purpose of ethanol is to play a dispersing role.

[0027] The organic amine described in step (2) is preferably at least one of triethylamine and hydrazine hydrate, preferably hydrazine hydrate.

[0028] The silane coupling agent described in step (2) is at least one of vinyl silane, amino silane, methacryloxy silane and epoxy silane, preferably γ-aminopropyltriethoxy silane.

[0029] The heating reflux time in step (2) is 10-15h.

[0030] The aging described in step (2) refers to aging at 150-180° C. for 2-6 hours.

[0031] A method for preparing the wear-resistant titanium alloy nano-injection polyester composite material comprises the following steps: mixing the components and extruding and granulating them through an extruder, wherein the granulation temperature is 240-270°C.

[0032] The above-mentioned wear-resistant titanium alloy nano-injection-molded polyester composite material is used in the preparation of mobile phone folding screen hinges and middle frame materials, especially in titanium alloy folding screen hinges and middle frame materials.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0034] (1) The polyester composite material provided by the present invention has a very high titanium alloy nano-injection molding bonding strength, which is greater than 35 MPa.

[0035] (2) The polyester composite material provided by the present invention has excellent wear resistance.

[0036] (3) The preparation method of the present invention is simple and easy to implement, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The schematic diagram of the structure of the titanium alloy plastic test piece is shown in FIG. 1 , titanium alloy part; and 2, plastic part.

[0038] Figure 2 This is the infrared spectrum of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours.

[0039] Figure 3 The actual pictures and scanning electron microscope pictures of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours, wherein (a) represents before calcination and (b) represents after calcination.

[0040] Figure 4 XRF elemental analysis characterization of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate in Example 2 before and after calcination at 800°C for 24 hours, wherein (a) represents before calcination and (b) represents after calcination. DETAILED DESCRIPTION

[0041] The present invention will be described in further detail below in conjunction with examples and accompanying drawings, but the embodiments of the present invention are not limited thereto. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0042] The details are as follows: PBT is Bluestar PBT1100, PET is Yizheng FG600, cylindrical glass fiber is Chongqing International ECS3031H, flat glass fiber is Chongqing International ECS307AT, ethylene methyl methacrylate glycidyl ether copolymer is Arkema AX8900, antioxidant 1010 is Tianjin Lianlong 1010, pentaerythritol tetrastearate (PETS) is purchased from Hubei Longxin Chemical Co., Ltd., calcium hypophosphite is purchased from Suzhou Lianxiong Chemical Co., Ltd., diethyl aluminum hypophosphite is Klein OP1230, and diethyl zinc hypophosphite is Klein OP590.

[0043] The wear resistance test in the following embodiments was conducted using the GBT3960-2016 standard method.

[0044] The titanium alloy nano-injection molding sample used in the present invention is prepared by the following process: Grade 5 titanium alloy material, size specifications, length 45mm, width 18mm, thickness 1.6mm; surface treatment process: sequentially immerse in NaOH solution alkaline washing (2mol / L, 50℃, 20 seconds), hydrochloric acid corrosion (1.5mol / L, 35℃, 40 seconds), and ammonia solution (2mol / L, 30℃, 4 minutes), and then the immersed sample is cleaned with water and dried to obtain a titanium alloy sample with nanopores on the surface.

[0045] Preparation of the plastic titanium alloy test monolith used in the present invention:

[0046] The present invention refers to the method of Japanese Dacheng nano injection molding related patent (US8057890 (B2)) to prepare the plastic metal test integral part. Figure 1 This is a schematic diagram of the structure of the titanium alloy plastic test piece. The size of the titanium alloy sheet is 18mm×45mm×1.6mm, the size of the plastic part is 10mm×45mm×3mm, and the bonding area between the plastic and the titanium alloy is 0.5cm 2 In all experiments, the injection molding maintained the same injection molding conditions, barrel temperature 260-300°C, mold temperature 150°C, and the plastic compound was injected onto the titanium alloy sheet to obtain a plastic titanium alloy test piece.

[0047] Plastic-metal bonding performance test:

[0048] The metal-plastic bonding strength test standard used in the present invention refers to the standard in the Japanese Daisei Chemical patent (US8057890 (B2)), and the plastic-metal bonding area is 0.5 cm 2 , a biaxial tensile test is performed on the test piece.

[0049] The preparation process of the plastic composite material is as follows: weigh the components in corresponding amounts according to weight percentage, then mix the components, and granulate the plastic composite using a twin-screw extruder at a granulation temperature of 240 to 320°C.

[0050] Example 1

[0051] Mix 100g of molybdenum disulfide, 400g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product A.

[0052] Example 2

[0053] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B.

[0054] The infrared spectra of the mixture of molybdenum disulfide, bismuth sulfide and copper sulfate before and after calcination at 800℃ for 24h are as follows Figure 2 As shown, the peak of SO4 at position 1197 disappears, indicating that the decomposition of copper sulfate at high temperature produces CuO and SO3; after high-temperature calcination, there is an obvious absorption peak at position 1080, indicating that metal persulfate components are generated. The high-temperature reaction process includes chemical reaction + physical doping process.

[0055] During the high temperature reaction, the mixture undergoes an obvious phase change. After calcination, the powdery white substance is not found when the image is magnified 1000 times, indicating that the copper sulfate is almost completely decomposed and copper oxide is generated at high temperature. Copper oxide and sulfide are physically doped, generating sulfide-doped copper oxide.

[0056] Example 2A

[0057] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of triethylamine, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B1.

[0058] Example 2B

[0059] Mix 250g of molybdenum disulfide, 250g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 20g of hydrazine hydrate, 40g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product B2.

[0060] Example 3

[0061] Mix 400g of molybdenum disulfide, 100g of bismuth sulfide and 500g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product C.

[0062] Example 4

[0063] Mix 400g of molybdenum disulfide, 400g of bismuth sulfide and 200g of copper sulfate, add to the reaction tube, and evacuate. Heat to 800℃ and keep for 24h. Cool naturally and take out the reactants. Grind the reactants into powder, add 2L of ethanol, 40g of hydrazine hydrate, and 20g of γ-aminopropyltriethoxysilane, and heat to reflux for 12h. Cool naturally, filter, and mature at 160℃ for 4h to obtain the final product D.

[0064] Example 5

[0065] This example aims to study the effects of different modified metal sulfides on the titanium alloy bonding and wear resistance of the polyester composite.

[0066] The polyester resin, the modified metal sulfide and other additives were mixed according to the weight percentages shown in Table 1, and extruded into granules by a twin-screw extruder at a granulation temperature of 240-270° C. The corresponding properties of the obtained polyester composite are shown in Table 1.

[0067] Table 1 Component weight percentage and performance data of polyester composites

[0068]

[0069] From the data in Table 1, it can be seen that when conventional wear-resistant additives PTFE or molybdenum disulfide are added, the bonding strength of titanium alloy NMT drops sharply. However, when suitable modified metal sulfide additives are added, the bonding strength of titanium alloy NMT of the material can be well maintained, and at the same time, the wear resistance is also greatly improved, especially in Test Example 6, which can obtain the best comprehensive performance.

[0070] Example 6

[0071] This example aims to study the effect of zinc diethylphosphite on the titanium alloy bonding and wear resistance of the polyester composite.

[0072] The polyester resin, diethyl zinc hypophosphite and other additives were mixed according to the weight percentages shown in Table 2, and extruded into granules by a twin-screw extruder at a granulation temperature of 240-270° C. The corresponding properties of the obtained polyester composite are shown in Table 2.

[0073] Table 2 Component weight percentage and performance data of polyester composites

[0074]

[0075] From the data in Table 2, it can be seen that although Test Example 6 has good wear resistance and high titanium alloy NMT bonding strength, its titanium alloy NMT bonding strength is still insufficient. The industry usually requires NMT bonding strength to reach 35MPa or more to achieve a high scale production success rate. When a certain amount of diethyl zinc hypophosphite is added to the system, the titanium alloy bonding strength can be greatly improved to reach the industry standard.

[0076] It can be seen from Test Examples 6 and 11-16 that as the amount of diethyl zinc hypophosphite increases, the bonding strength of the titanium alloy first increases and then decreases, and when the weight percentage of diethyl zinc hypophosphite exceeds 0.5%, the mass wear also increases, that is, when the weight percentage of diethyl zinc hypophosphite is 0.2-0.5%, better bonding strength and mass wear of the titanium alloy can be achieved at the same time.

[0077] From the comparison between Test Example 13 and Test Example 14, it can be seen that when flat glass fibers are used, the resulting composite material has higher wear resistance and higher bonding strength to titanium alloy than cylindrical glass fibers.

[0078] From the comparison between Test Example 13 and Test Examples 17-18, it can be seen that when analogs of diethyl zinc hypophosphite such as diethyl aluminum hypophosphite and calcium hypophosphite are used, similar effects cannot be achieved.

[0079] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A wear-resistant titanium alloy nano-injection polyester composite material, Features The composition comprises the following components in weight percentage: PBT 25%-60%; PET 10-30%; Modified metal sulfide 1%-10%; Zinc diethyl hypophosphite 0.2%-0.5%; Toughening agent 1%-10%; Glass fiber 10%-50%; The modified metal sulfide is prepared by the following method: (1) Molybdenum disulfide, bismuth sulfide and copper sulfate are mixed, vacuumized, and then heated for reaction. After the reaction is completed, the mixture is naturally cooled, and the reaction product is taken out and ground into powder; (2) mixing the reaction product ground in step (1), a monohydric alcohol, an organic amine, and a silane coupling agent, and then heating and refluxing the mixture for reaction. After the reaction is completed, the mixture is naturally cooled, filtered, and then heated and aged to obtain a modified metal sulfide. In the preparation process of the modified metal sulfide, the amounts of the five raw materials used meet the following requirements: the mass ratio of molybdenum disulfide, bismuth sulfide, copper sulfate, organic amine, and silane coupling agent is 20-30:20-30:40-60:3-5:1-3; The heating reaction in step (1) refers to heating to 700-900°C and maintaining for 12-36 hours; The aging described in step (2) refers to aging at 150-180° C. for 2-6 hours.

2. The wear-resistant titanium alloy nano-injection polyester composite material according to claim 1, Features: The wear-resistant titanium alloy nano-injection polyester composite material further comprises at least one of an antioxidant and a release agent, wherein the weight percentage of the antioxidant is 0.05%-0.5%, and the weight percentage of the release agent is 0.1%-2.0%.

3. The wear-resistant titanium alloy nano-injection polyester composite material according to claim 1, Features: The weight percentage of the modified metal sulfide in the wear-resistant titanium alloy nano-injection polyester composite material is 4-6%.

4. The wear-resistant titanium alloy nano-injection polyester composite material according to claim 1, Features: The glass fiber is cylindrical glass fiber or flat glass fiber; The toughening agent is a copolymerized glycidyl ether toughening agent.

5. The wear-resistant titanium alloy nano-injection polyester composite material according to claim 1, Features: The heating reflux time in step (2) is 10-15 hours.

6. The wear-resistant titanium alloy nano-injection polyester composite material according to claim 1, Features: The monohydric alcohol described in step (2) refers to at least one of the monohydric alcohols with less than 6 carbon atoms; The organic amine in step (2) is at least one of triethylamine and hydrazine hydrate; The silane coupling agent described in step (2) is at least one of vinyl silane, amino silane, methacryloxy silane and epoxy silane.

7. A method for preparing the wear-resistant titanium alloy nano-injection polyester composite material according to any one of claims 1 to 6, Features The following steps are involved: The components are mixed and extruded into granules by an extruder, and the granulation temperature is 240-270°C.

8. Use of the wear-resistant titanium alloy nano-injection-molded polyester composite material according to any one of claims 1 to 6 in the preparation of mobile phone folding screen hinges and middle frame materials.

Citation Information

Patent Citations

  • Composite of aluminum alloy and resin and manufacturing method thereof

    US8057890B2

  • Composite of metal with resin and process for producing the same

    WO2007040245A1

  • Heat-conduction and abrasion-resistance high-strength polyphenylene sulfide composite and preparing method thereof

    CN106084778A

  • Sulfide coated particle as well as preparation method and application thereof

    CN107983272A