A light-heat synergistic catalyst for liquid phase selective oxidation reaction and a one-step synthesis method thereof

The composite metal silicate catalyst is prepared through a one-step synthesis method, which solves the problems of complexity and high cost in the preparation of existing photo-thermal synergistic catalysts, achieves efficient and stable liquid-phase selective oxidation reactions of hydrocarbons, and improves catalytic performance and products. Yield.

CN117566751BActive Publication Date: 2024-10-29HUAIBEI NORMAL UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311530334.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2024-10-29
Estimated Expiration
2043-11-16

AI Technical Summary

Technical Problem

The preparation method of the existing photo-thermal synergistic catalyst is complicated, which increases the synthesis steps and equipment costs, limiting its industrial application in the liquid-phase selective oxidation reaction of hydrocarbons.

Method used

Using a one-step synthesis method, a silicon source, a metal source, an alkali source and a commercially available organic template are mixed, and a composite metal silicate catalyst is prepared through steps such as stirring, crystallization, washing, and roasting to form a photocatalytic and thermocatalytic activity. Three-dimensional crystal skeleton for catalyzing liquid-phase selective oxidation of hydrocarbons.

Benefits of technology

It achieves high oxidation product yield, mild reaction conditions, low-cost preparation, good catalytic stability and adjustable light-thermal synergistic catalytic performance, which significantly improves the catalytic performance, especially the yield of the target product at low temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117566751B_ABST
    Figure CN117566751B_ABST
Patent Text Reader

Abstract

The present invention discloses a light-heat synergistic catalyst for liquid phase selective oxidation reaction and a one-step synthesis method thereof, which is characterized in that a commercially available organic template is used to prepare a three-dimensional crystal framework with silicon and oxygen as main elements, and a metal oxide site with photocatalytic and thermal catalytic activity is in situ generated and compounded, and the chemical composition is M m n+ N p q+ SiO x The composite metal silicate catalyst is used to catalyze the liquid phase selective oxidation reaction of hydrocarbons to prepare corresponding high value-added oxygen-containing chemicals. Compared with the prior art, the present invention has fewer preparation steps and lower preparation costs, can effectively adjust the number and state of photocatalytic and thermal catalytic active sites, and significantly improves the liquid phase selective oxidation performance of hydrocarbons in the catalytic light-heat synergistic system, showing a higher target product yield at a lower temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemical synthesis and chemical application, and in particular to a composite metal silicate catalyst for light-heat synergistic catalytic liquid phase selective oxidation reaction and a one-step synthesis method thereof. Background Art

[0002] At present, the production process of functional hydrocarbons based on hydrocarbon-based chemicals mainly relies on thermal energy support, and the pressure on the environment caused by the conversion of non-renewable energy to thermal energy has greatly promoted the innovation of the energy system. Light energy is inexhaustible, and photocatalytic technology has become a research hotspot in the field of organic synthesis due to its environmental friendliness and low energy consumption. However, this attractive technology is still far from actual industrial application, and the national light energy utilization rate is less than 1%. From the perspective of practical application, building an efficient light-heat composite catalytic system and using clean light energy to compensate for part of the thermal energy is expected to truly realize the effective use of light energy in the production process and promote the construction of a cleaner chemical energy system.

[0003] More than 60% of the production processes of chemicals involve the selective oxidation of hydrocarbons. The skeleton metal sites on heteroatom silicates represented by TS-1 (MFI topology, Titanium Silicalite-1) can activate oxidants (such as oxygen, hydrogen peroxide, cumene hydroperoxide, etc.) and realize the transfer process of active oxygen (US Patent 1983, 4410501), and the three-dimensional pore structure can achieve product selectivity regulation through the shape-selective confinement of guest molecules. This makes heteroatom silicates not only have excellent catalytic activity in thermal energy-driven liquid-phase selective oxidation systems, but also have the potential to construct efficient light-heat synergistic catalysts. According to literature reports, by doping heteroatom silicates with photoresponsive photocatalytic active sites, a composite catalyst suitable for light-heat synergistic catalytic liquid-phase selective oxidation reactions can be constructed (Appl. Catal. BEnviron., 2018, 12, 237, 660). However, the current preparation methods of photo-thermal synergistic catalysts often adopt a post-doping method, that is, synthesizing the corresponding photocatalyst and thermal catalyst separately and then doping and compounding them (Mol. Catal., 2019, 8, 473, 110389), which increases the synthesis steps and equipment costs, limiting its industrial application. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a light-heat synergistic catalyst for liquid-phase selective oxidation reactions and a one-step synthesis method thereof. A commercially available organic template is used to prepare a three-dimensional crystal skeleton with silicon and oxygen as the main elements, while in situ generating and compounding metal active sites with photocatalytic and thermocatalytic activities, which are used to catalyze the liquid-phase selective oxidation reaction of hydrocarbons. The catalyst has a high yield of oxidation products, mild reaction conditions, environmental friendliness, and good catalytic stability. The preparation process has few steps and low preparation cost, and the number and state of photocatalytic and thermocatalytic active sites can be effectively adjusted. The liquid-phase selective oxidation performance of hydrocarbons in the catalytic light-heat synergistic system is significantly improved, showing a higher yield of target products at lower temperatures.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] The present invention first provides a one-step synthesis method of a light-heat synergistic catalyst for liquid phase selective oxidation reaction, which is characterized in that a silicon source, a metal source, an alkali source, a commercially available organic template and deionized water are mixed, stirred at a temperature of 15 to 150° C. for 0.5 to 8 hours, and then crystallized for 1 to 8 days. After the crystallization, the product is washed, filtered, dried, and calcined at a temperature of 300 to 750° C. for 3 to 10 hours to obtain a composite metal silicate catalyst, which is a light-heat synergistic catalyst for liquid phase selective oxidation reaction.

[0007] Furthermore, the silicon source is calculated as SiO2, the metal source is calculated as M m n+ O, alkali source is N p q+ The molar ratio of O to commercially available organic template and deionized water is 0.4-0.9:0.02-0.5:0-0.4:0.01-1.0:2-200, wherein: M is the metal in the metal source, m is the molar ratio of the metal ion in the metal source to Si in the silicon source, and n is the valence of M; N is the metal ion in the alkali source, p is the molar ratio of the metal ion in the alkali source to Si in the silicon source, and q is the valence of N.

[0008] Further: the silicon source is at least one of tetraethyl silicate, silica sol, fumed silica, white carbon black, water glass, silica microspheres and molecular sieves; the metal source is at least one of oxides, sulfates, nitrates, phosphates, carbonates, chlorides or metal-containing organic matter of aluminum, titanium, tin, cobalt and / or zinc; the alkali source is at least one of sodium hydroxide, sodium metaaluminate, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate and potassium bicarbonate; the organic template is a quaternary ammonium salt or quaternary ammonium base form of a compound having a structural formula as shown in formula (A), or at least one of a compound having a structural formula as shown in formula (B):

[0009]

[0010] In formula (A): R1, R2, R3 and R4 are each independently selected from a linear or cyclic C 1-10 Alkyl, preferably C 1-5 alkyl;

[0011]

[0012] In formula (B): R5, R6 and R7 are each independently selected from a linear or cyclic C 1-10 Alkyl, preferably C 1-6 alkyl.

[0013] Further, the topological structure of the molecular sieve that can be used as a silicon source includes at least one of MFI, *BEA, MWW, MOR, FAU and FER.

[0014] Furthermore, the method for achieving the crystallization includes at least one of heating, ultrasound, light irradiation and microwaves.

[0015] Further, the quaternary ammonium salt form of the compound shown in formula (A) has a quaternary nitrogen (N + The counter anion of the structure is a halogen ion (such as Cl - Br - ,I - etc.); a quaternary ammonium base form of a compound having a structural formula as shown in formula (A), wherein the quaternary nitrogen (N + The counter anion of the structure is the hydroxide ion (OH - ).

[0016] The composite metal silicate catalyst prepared by the one-step synthesis method of the present invention uses silicon and oxygen as main elements connected in tetrahedral form to form a three-dimensional crystal framework of metal oxide sites with photocatalytic and thermal catalytic activity, and its chemical composition is M m n+ N p q+ SiO x ; Wherein, M is the metal in the metal source, m is the molar ratio of the metal ions in the metal source to Si in the silicon source, and n is the valence of M; N is the metal ions in the alkali source, p is the molar ratio of the metal ions in the alkali source to Si in the silicon source, and q is the valence of N; x is the molar ratio of O to Si, and x = (m×n+p×q+4) / 2.

[0017] The second purpose of the present invention is to provide the composite metal silicate prepared as a catalyst for catalyzing the liquid-phase selective oxidation reaction of hydrocarbons in a photothermal synergistic system to synthesize high value-added oxygen-containing compounds. The specific method is: mixing the composite metal silicate catalyst with a hydrocarbon compound and a solvent, adding an oxidant to a reactor, stirring the reaction at 20 to 140°C under ultraviolet light for 0.5 to 5 hours, and removing the catalyst by filtration after the reaction. The filtrate is separated and purified to obtain a hydrocarbon oxide; the weight ratio of the hydrocarbon compound, the solvent and the composite metal silicate catalyst is 1:0 to 20:0.02 to 0.35.

[0018] Furthermore: the solvent is methanol, ethanol, propanol, isopropanol, butanol, tert-butanol, acetonitrile, acetone, n-hexane, cyclohexane or deionized water; the oxidant is oxygen, a mixed gas containing oxygen, an aqueous hydrogen peroxide solution, tert-butyl hydroperoxide or isopropylbenzene hydroperoxide; the hydrocarbon compound is at least one of straight-chain alkanes and straight-chain olefins with a carbon number of 1 to 10 and cyclic alkanes and cyclic olefins with a carbon number of 1 to 10.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] The composite metal silicate catalyst of the present invention has high photo-thermal composite catalytic selective oxidation performance and oxygen-containing compound yield, milder reaction conditions, good catalytic stability, adopts a one-step synthesis method, and the preparation process is simpler, more efficient and low-cost. It can effectively adjust the number and state of photocatalytic and thermal catalytic active sites, and has significantly improved performance when catalyzing the liquid-phase selective oxidation reaction of hydrocarbon compounds in a photo-thermal composite system, showing a high yield of the target oxygen-containing compound at a low reaction temperature, further broadening the research and application fields of photo-thermal composite catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of the composite metal silicate prepared in Example 1;

[0022] Figure 2 The UV-visible absorption spectrum of the metal silicate prepared in Example 1;

[0023] Figure 3 The X-ray diffraction pattern of the composite metal silicate prepared in Example 2;

[0024] Figure 4 is a transmission electron microscope image of the composite metal silicate prepared in Example 2, and the inset is its electron diffraction pattern;

[0025] Figure 5 This is a transmission electron microscopy image of the composite metal silicate prepared in Example 3;

[0026] Figure 6 This is a transmission electron microscopy image of the composite metal silicate prepared in Example 4. DETAILED DESCRIPTION

[0027] The present invention comprises mixing a silicon source, a metal source, an alkali source, a commercially available organic template and deionized water, stirring at a temperature of 15 to 150° C. for 0.5 to 8 hours, and then crystallizing for 1 to 8 days. After the crystallization, the product is washed, filtered, dried, and calcined at a temperature of 300 to 750° C. for 3 to 10 hours to prepare a three-dimensional crystal framework having silicon and oxygen as main elements connected in a tetrahedral form and compounding metal oxide sites with photocatalytic and thermal catalytic activity, wherein the chemical composition is M m n+ N p q+ SiO x , wherein: M is the metal in the metal source (selected from at least one of aluminum, titanium, tin, cobalt, and zinc), m is the molar ratio of the metal ion in the metal source to Si in the silicon source, and n is the valence of M; N is the metal ion in the alkali source (selected from at least one of lithium ion, sodium ion, potassium ion, magnesium ion, calcium ion, and hydrogen ion), p is the molar ratio of the metal ion in the alkali source to Si in the silicon source, and q is the valence of N; x is the molar ratio of O to Si, and x=(m×n+p×q+4) / 2.

[0028] The preparation and application of the present invention are further described below through specific examples:

[0029] Example 1

[0030] Fuming silica gel (in terms of SiO2), potassium carbonate (in terms of K2O), tetrabutyl titanate (in terms of TiO2), an organic template A (R1, R2, R3 are selected from methyl, R4 is selected from adamantyl, and the counter anion is selected from OH) as shown in formula (A) - , i.e. N,N,N-trimethyl-1-adamantyl ammonium hydroxide), an organic template B (R1 and R2 are cyclohexyl groups, R3 is hydrogen, i.e. dicyclohexylamine) having a structural formula as shown in formula (B) and deionized water are mixed in a molar ratio of 0.9:0.08:0.5:0.25:0.3:33.5, stirred at 25°C for 6 hours, then crystallized at 150°C for 5 days, and the crystallized product is washed, filtered, dried, and calcined at 600°C for 6 hours to obtain a composite metal silicate.

[0031] See also Figure 1 The composite metal silicate prepared in Example 1 was shown to have a thin-sheet stacking morphology by scanning electron microscopy.

[0032] See also Figure 2The UV-visible absorption spectrum of the composite metal silicate prepared in Example 1 shows the presence of framework tetracoordinated titanium species and anatase species in the sample.

[0033] Example 2

[0034] 30wt.% silica sol aqueous solution (in terms of SiO2), sodium hydroxide (in terms of Na2O), tetrabutyl titanate (in terms of TiO2), an organic template A (R1, R2, R3, R4 are propyl groups, and the counter anion is OH) as shown in formula (A) are added. - , i.e. tetrapropylammonium hydroxide) and deionized water are mixed in a molar ratio of 1.0:0.05:0.4:0.35:13.1, stirred at 75°C for 6 hours, then crystallized at 170°C for 3 days, and the crystallized product is washed, filtered, dried, and calcined at 600°C for 6 hours to obtain a composite metal silicate.

[0035] See also Figure 3 The X-ray diffraction pattern of the composite metal silicate prepared in Example 2 shows good crystallinity.

[0036] See also Figure 4 The composite metal silicate prepared in Example 2 was shown to be a nanomaterial of about 40 nm by transmission electron microscopy.

[0037] Example 3

[0038] All-silicon MFI molecular sieve (in terms of SiO2), sodium bicarbonate (in terms of Na2O), titanium sulfate (in terms of TiO2), an organic template A (R1, R2, R3, R4 are selected from ethyl, and the counter anion is selected from OH) as shown in formula (A) - , i.e. tetraethylammonium hydroxide) and deionized water were mixed in a molar ratio of 1.0:0.12:0.45:0.25:35.0, stirred at 25°C for 1 hour, and then microwave-assisted crystallization for 12 hours. The crystallized product was washed, filtered, dried, and calcined at 550°C for 6 hours to obtain a composite metal silicate.

[0039] See also Figure 5 The composite metal silicate prepared in Example 3 was shown to be a nanomaterial of about 65 nm by transmission electron microscopy.

[0040] Example 4

[0041] Tetraethyl orthosilicate (in terms of SiO2), sodium hydroxide (in terms of Na2O), tin chloride (in terms of SnO2), an organic template A (R1, R2, R3, R4 are selected as ethyl, and the counter anion is selected as OH) as shown in formula (A) -, i.e. tetraethylammonium hydroxide) and deionized water are mixed in a molar ratio of 1.0:0.1:0.35:0.5:7.5, stirred at 100°C for 1 hour, then crystallized at 140°C for 1 day, and the crystallized product is washed, filtered, dried, and calcined at 600°C for 6 hours to obtain a composite metal silicate.

[0042] See also Figure 6 The composite metal silicate prepared in Example 4 showed a flower-like cluster morphology under transmission electron microscopy.

[0043] Example 5

[0044] High silicon * BEA molecular sieve (in terms of SiO2), sodium aluminate (in terms of Na2O), zinc nitrate (in terms of ZnO), an organic template A (R1 and R2 are selected as propyl, R3 and R4 are selected as methyl, and the counter anion is selected as OH) as shown in formula (A) - , i.e. dimethyldipropylammonium hydroxide) and deionized water are mixed in a molar ratio of 1.0:0.08:0.32:0.53:12.0, stirred at 25°C for 1 hour, then ultrasonically crystallized at 80°C for 8 hours, and the crystallized product is washed, filtered, dried, and calcined at 650°C for 6 hours to obtain a composite metal silicate.

[0045] Example 6

[0046] White carbon black (in terms of SiO2), potassium hydroxide (in terms of K2O), tin tetrachloride (in terms of SnO2), an organic template A (R1, R2, R3 are butyl, R4 is methyl, and the counter anion is I) as shown in formula (A) are added. - , i.e. tributyl methyl ammonium iodide), an organic template B (R1 and R2 are cyclohexyl groups, R3 is hydrogen, i.e. dicyclohexylamine) having a structural formula as shown in formula (B) and deionized water are mixed in a molar ratio of 1.0:0.03:0.4:0.22:0.34:41.1, stirred at 25°C for 6 hours, then crystallized at 160°C for 4 days, and the crystallized product is washed, filtered, dried, and calcined at 600°C for 5 hours to obtain a composite metal silicate.

[0047] Example 7

[0048] Tetraethyl orthosilicate (in terms of SiO2), sodium carbonate (in terms of Na2O), titanium trichloride (in terms of TiO2), an organic template A (R1, R2, R3, R4 are propyl groups, and the counter anion is Br) as shown in formula (A) are added. -, i.e. tetrapropylammonium bromide) and deionized water are mixed in a molar ratio of 1.0:0.05:0.42:0.41:15.0, stirred at 60°C for 5 hours, then crystallized at 140°C for 2 days, and the crystallized product is washed, filtered, dried, and calcined at 600°C for 6 hours to obtain a composite metal silicate.

[0049] Example 8

[0050] The composite metal silicate catalyst prepared in the above Example 1 was applied to the cyclohexane oxidation reaction to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 0.5 g of the composite metal silicate catalyst and 8.4 g of cyclohexane were sequentially added to a photocatalytic reactor and mixed, oxygen was introduced into the reaction liquid to replace the air in the reactor, and the reactor pressure was adjusted to 0.5 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 120°C under light for 1 hour. The reaction liquid was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain oxidation products cyclohexanone and cyclohexanol.

[0051] The above products were analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of the oxidation product was 21.1%, and the proportions of cyclohexanone and cyclohexanol in the product were 40.5% and 59.5%, respectively.

[0052] The catalytic activity comparison between the composite metal silicate prepared in Example 1 and the TS-1 titanosilicate is shown in Table 1 below:

[0053] Table 1 Comparison of catalytic activity between composite metal silicate and TS-1 titanosilicate

[0054] catalyst Oxide yield (%) Cyclohexanone selectivity (%) Cyclohexanol selectivity (%) Composite metal silicate 21.1% 40.5% 59.5% TS-1 Titanosilicate 4.2% 47.9% 52.1%

[0055] The above-mentioned TS-1 titanosilicate catalyst was synthesized according to the method of patent (CN112978747A), with a Si / Ti molar ratio of 40. The reaction conditions for its use as a catalyst in the cyclohexane oxidation reaction were the same as those in Example 8. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0056] Example 9

[0057] The composite metal silicate catalyst prepared in the above Example 1 was applied to the cyclohexane oxidation reaction to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 0.5 g of the composite metal silicate catalyst and 11.4 g of cyclohexane were added to the photocatalytic reactor in sequence and mixed, oxygen was introduced into the reaction liquid to replace the air in the reactor, and the reactor pressure was adjusted to 0.5 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 95°C under light for 1.5 hours. The reaction liquid was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain oxidation products cyclohexanone and cyclohexanol.

[0058] The above products were analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of the oxidation product was 17.9%, and the proportions of cyclohexanone and cyclohexanol in the product were 41.3% and 58.7%, respectively.

[0059] The catalytic activity comparison between the composite metal silicate prepared in Example 1 and the TS-1 titanosilicate is shown in Table 2 below:

[0060] Table 2 Comparison of catalytic activity between composite metal silicate and TS-1 titanosilicate

[0061] catalyst Oxide yield (%) Cyclohexanone selectivity (%) Cyclohexanol selectivity (%) Composite metal silicate 17.9% 41.3% 58.7% TS-1 Titanosilicate 2.7% 48.6% 51.4%

[0062] The above-mentioned TS-1 titanosilicate catalyst was synthesized according to the patent (CN112978747A) method, with a Si / Ti molar ratio of 40. The reaction conditions for its use as a catalyst in the cyclohexane oxidation reaction were the same as those in Example 9. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0063] Example 10

[0064] The composite metal silicate catalyst prepared in the above Example 3 was applied to the cyclohexane oxidation reaction to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 1.0 g of the composite metal silicate catalyst and 8.4 g of cyclohexane were sequentially added to a photocatalytic reactor and mixed, air was introduced into the reaction solution, and the reactor pressure was adjusted to 1.0 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 100°C under light for 1 hour. The reaction solution was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain oxidation products cyclohexanone and cyclohexanol.

[0065] The above products were analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of the oxidation product was 29.4%, and the proportions of cyclohexanone and cyclohexanol in the product were 43.3% and 56.7%, respectively.

[0066] The catalytic activity comparison between the composite metal silicate prepared in Example 3 and the composite semiconductor material is shown in Table 3 below:

[0067] Table 3 Comparison of catalytic activity between composite metal silicate and Mn3O4 / CdZnS

[0068] catalyst Oxide yield (%) Cyclohexanone selectivity (%) Cyclohexanol selectivity (%) Composite metal silicate 29.4% 43.3% 56.7% <![CDATA[Mn3O4 / CdZnS]]> 12.2% 48.5% 51.5%

[0069] The above-mentioned Mn3O4 / CdZnS catalyst was synthesized with reference to the method of Appl.Surf.Sci., 2022, 3,579, 151978, and the reaction conditions for its use as a catalyst in the cyclohexane oxidation reaction were the same as those in Example 10. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0070] Embodiment 11

[0071] The composite metal silicate catalyst prepared in the above Example 1 was applied to the cyclohexane oxidation reaction to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 1.5 grams of the composite metal silicate catalyst and 12.8 grams of cyclohexane were added to the photocatalytic reactor in sequence and mixed, oxygen was introduced into the reaction liquid to replace the air in the reactor, and the reactor pressure was adjusted to 0.5 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 100°C under light for 1 hour. The reaction liquid was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain oxidation products cyclohexanone and cyclohexanol.

[0072] The above products were analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of the oxidation product was 32.5%, and the proportions of cyclohexanone and cyclohexanol in the product were 39.5% and 60.5%, respectively.

[0073] The catalytic activity comparison between the composite metal silicate prepared in Example 1 and the composite semiconductor material is shown in Table 4 below:

[0074] Table 4 Comparison of catalytic activity between composite metal silicate and Cr2O3-Al2O3

[0075] catalyst Oxide yield (%) Cyclohexanone selectivity (%) Cyclohexanol selectivity (%) Composite metal silicate 21.1% 40.5% 59.5% <![CDATA[Cr2O3-Al2O3]]> 8.7% 38.9% 61.1%

[0076] The above-mentioned Cr2O3-Al2O3 catalyst was synthesized according to the method of ACS Appl. Mater. Interfaces, 2020, 12, 22531. The reaction conditions for its use as a catalyst in the cyclohexane oxidation reaction were the same as those in Example 11. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0077] Example 12

[0078] The composite metal silicate catalyst prepared in the above Example 2 was applied to the epoxidation reaction of 1-hexene to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 0.5 g of the composite metal silicate catalyst, 79 g of methanol and 8.4 g of 1-hexene were added to the photocatalytic reactor in sequence and mixed, oxygen was introduced into the reaction liquid to replace the air in the reactor, and the reactor pressure was adjusted to 0.4 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 60°C under light for 2 hours. The reaction liquid was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain the oxidation product 1,2-epoxyhexane.

[0079] The above product was analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of 1,2-epoxyhexane was 5.1% and the selectivity was 90.7%.

[0080] The catalytic activity comparison between the composite metal silicate prepared in Example 2 and the TS-1 titanosilicate is shown in Table 5 below:

[0081] Table 5 Comparison of catalytic activity between composite metal silicate and TS-1 titanosilicate

[0082] catalyst Yield of 1,2-epoxyhexane (%) 1,2-Epoxyhexane selectivity (%) Composite metal silicate 5.1% 90.7% TS-1 Titanosilicate 0.5% 75.8%

[0083] The above-mentioned TS-1 titanosilicate catalyst was synthesized according to the patent method (CN112978747A), with a Si / Ti molar ratio of 40. The reaction conditions for its use as a catalyst in the epoxidation reaction of 1-hexene were the same as those in Example 12. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0084] Embodiment 13

[0085] The composite metal silicate catalyst prepared in the above Example 1 was applied to the epoxidation reaction of 1-hexene to characterize its catalytic activity under the light-heat composite system. The specific application is as follows: 0.5 g of the composite metal silicate catalyst, 79 g of methanol and 8.4 g of 1-hexene were added to the photocatalytic reactor in sequence and mixed, oxygen was introduced into the reaction liquid to replace the air in the reactor, and the reactor pressure was adjusted to 0.5 MPa and kept constant, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 45°C under light for 2 hours. The reaction liquid was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain the oxidation product 1,2-epoxyhexane.

[0086] The above product was analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of 1,2-epoxyhexane was 3.4% and the selectivity was 87.9%.

[0087] The catalytic activity comparison between the composite metal silicate prepared in Example 1 and the TS-1 titanosilicate is shown in Table 6 below:

[0088] Table 6 Comparison of catalytic activity between composite metal silicate and TS-1 titanosilicate

[0089] catalyst Yield of 1,2-epoxyhexane (%) 1,2-Epoxyhexane selectivity (%) Composite metal silicate 3.4% 87.9% TS-1 Titanosilicate 0.2% 79.4%

[0090] The above-mentioned TS-1 titanosilicate catalyst was synthesized according to the patent method (CN112978747A), with a Si / Ti molar ratio of 40. The reaction conditions for its use as a catalyst in the epoxidation reaction of 1-hexene were the same as those in Example 13. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0091] Embodiment 14

[0092] The composite metal silicate catalyst prepared in the above Example 7 was applied to the epoxidation reaction of 1-hexene to characterize its catalytic activity under the light-heat composite system. The specific application was as follows: 1.0 g of the composite metal silicate catalyst, 79 g of methanol and 11.4 g of 1-hexene were added to a photocatalytic reactor in sequence and mixed, and 10.9 g of an aqueous hydrogen peroxide solution (27.5 wt.%) was added, the reactor was transferred to a constant temperature water bath, and the reaction was stirred at 60° C. under light for 2 hours. The reaction solution was filtered to separate the solid catalyst, and the filtrate was separated and purified to obtain the oxidation product 1,2-epoxyhexane.

[0093] The above product was analyzed by gas chromatography (Shimadzu 2014, FID), and the yield of 1,2-epoxyhexane was 33.7% and the selectivity was 94.2%.

[0094] The catalytic activity comparison between the composite metal silicate prepared in Example 7 and the TS-1 titanosilicate is shown in Table 7 below:

[0095] Table 7 Comparison of catalytic activity between composite metal silicate and TS-1 titanosilicate

[0096] catalyst Yield of 1,2-epoxyhexane (%) 1,2-Epoxyhexane selectivity (%) Composite metal silicate 33.7% 94.2% TS-1 Titanosilicate 18.6% 93.1%

[0097] The above-mentioned TS-1 titanosilicate catalyst was synthesized according to the patent method (CN112978747A), with a Si / Ti molar ratio of 40. The reaction conditions for its use as a catalyst in the epoxidation reaction of 1-hexene were the same as those in Example 14. Gas chromatography analysis of the two catalysts showed that the catalytic activity of the composite metal silicate prepared by the present invention in the light-heat synergistic cyclohexane oxidation reaction was significantly improved.

[0098] The protection content of the present invention is not limited to the above embodiments. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention and are protected by the attached claims.

Claims

1. A one-step synthesis method of a light-heat synergistic catalyst for liquid phase selective oxidation reaction, characterized in that: A silicon source, a metal source, an alkali source, a commercially available organic template and deionized water are mixed, stirred at a temperature of 15 to 150° C. for 0.5 to 8 hours, and then crystallized for 1 to 8 days. The product after the crystallization is washed, filtered, dried, and calcined at a temperature of 300 to 750° C. for 3 to 10 hours to obtain a composite metal silicate catalyst, which is a light-heat synergistic catalyst for liquid phase selective oxidation reaction; the composite metal silicate catalyst uses silicon and oxygen as main elements connected in a tetrahedral form to form a three-dimensional crystal framework of metal oxide sites with photocatalytic and thermal catalytic activities, and its chemical composition is ; wherein M is the metal in the metal source, m is the molar ratio of the metal ion in the metal source to Si in the silicon source, n is the valence of M; N is the metal ion in the alkali source, p is the molar ratio of the metal ion in the alkali source to Si in the silicon source, q is the valence of N; x is the molar ratio of O to Si, and ; The silicon source is measured in SiO2, the metal source is measured in M m n+ O, alkali source is N p q+ The molar ratio of the silicon source to the commercially available organic template and deionized water is 0.4-0.9: 0.32-0.5: 0-0.4: 0.01-1.0: 2-200, wherein: M is the metal in the metal source, m is the molar ratio of the metal ion in the metal source to Si in the silicon source, and n is the valence of M; N is the metal ion in the alkali source, p is the molar ratio of the metal ion in the alkali source to Si in the silicon source, and q is the valence of N; The silicon source is at least one of tetraethyl silicate, silica sol, fumed silica, white carbon black, water glass, silica microspheres and molecular sieves; the metal source is at least one of titanium oxide, sulfate, nitrate, phosphate, carbonate, chloride or titanium-containing organic matter; the alkali source is at least one of sodium hydroxide, sodium metaaluminate, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate and potassium bicarbonate; the organic template is a quaternary ammonium salt or quaternary ammonium base form of the compound represented by structural formula (A), or at least one of the compounds represented by structural formula (B): (A) In formula (A): R1, R2, R3 and R4 are each independently selected from a linear or cyclic C 1-10 alkyl; (B) In formula (B): R5, R6 and R7 are each independently selected from a linear or cyclic C 1-10 alkyl.

2. The one-step synthesis method according to claim 1, characterized in that: The topological structures of molecular sieves that can be used as silicon sources include MFI, , MWW, MOR, FAU and FER.

3. The one-step synthesis method according to claim 1, characterized in that: The crystallization is achieved by at least one of heating, ultrasound, light and microwaves.

4. The one-step synthesis method according to claim 2, characterized in that: The quaternary ammonium salt form of the compound represented by structural formula (A) has a quaternary nitrogen N + The balanced anion of the structure is a halogen ion; the quaternary ammonium base form of the compound shown in structural formula (A) has a quaternary nitrogen N + The counter anion of the structure is the hydroxide ion.

5. A composite metal silicate catalyst obtained by the one-step synthesis method according to any one of claims 1 to 4.

6. An application of the composite metal silicate catalyst according to claim 5, characterized in that: The composite metal silicate catalyst is used for the liquid phase selective oxidation reaction of hydrocarbons in a light-heat synergistic system.

7. The use according to claim 6, characterized in that: The specific application method of the composite metal silicate catalyst is as follows: the composite metal silicate catalyst is mixed with a hydrocarbon compound and a solvent, an oxidant is added to a reactor, and the mixture is stirred and reacted at 20 to 140° C. for 0.5 to 5 hours under ultraviolet light. After the reaction is completed, the catalyst is removed by filtration, and the filtrate is separated and purified to obtain a hydrocarbon oxide; the weight ratio of the hydrocarbon compound, the solvent and the composite metal silicate catalyst is 1:0 to 20:0.02 to 0.

35.

8. The use according to claim 7, characterized in that: The solvent is methanol, ethanol, propanol, isopropanol, butanol, tert-butanol, acetonitrile, acetone, n-hexane, cyclohexane or deionized water; the oxidant is oxygen, a mixed gas containing oxygen, an aqueous hydrogen peroxide solution, tert-butyl hydroperoxide or isopropylbenzene hydroperoxide; the hydrocarbon compound is at least one of a straight-chain alkane with a carbon number of 1 to 10, a straight-chain olefin with a carbon number of 1 to 10, a cyclic alkane with a carbon number of 1 to 10, and a cyclic olefin with a carbon number of 1 to 10.

Citation Information

Patent Citations

  • Nanometer titanium silicalite molecular sieve TS-1 as well as preparation method and application thereof

    CN112978747A

  • A composite titanium aluminosilicate catalyst, its preparation method and application

    CN114931974A