Antibacterial and environmentally friendly polypropylene composite plastic and preparation method thereof
By combining graphene oxide-loaded zinc oxide and nano-zinc oxide into polypropylene plastic, the problems of antibacterial properties and degradation difficulties of polypropylene plastic were solved, and the preparation of highly efficient antibacterial and degradable composite plastics was achieved.
Patent Information
- Application Number
- CN202311595797.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-11-24
AI Technical Summary
Existing polypropylene plastics do not have antibacterial properties, and inorganic antibacterial agents make the plastics difficult to degrade, posing safety hazards. Furthermore, nano zinc oxide has poor dispersibility in polypropylene, affecting the antibacterial effect and plastic properties.
A high-strength composite material was prepared by combining graphene oxide-supported zinc oxide with nano-zinc oxide, and by grafting pretreated graphene oxide with dendritic polyamide amine through surface deposition of zinc oxide. This composite material was then mixed with SBS latex and a dispersant and prepared using a twin-screw extruder.
It achieves long-lasting and stable antibacterial effects, enhances the mechanical properties of plastics, and promotes their degradation in the environment, making it suitable for large-scale application.
Smart Images

Figure CN117586578B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antibacterial plastics, and in particular to an antibacterial and environmentally friendly polypropylene composite plastic and a preparation method thereof. Background Art
[0002] Polypropylene is a thermoplastic synthetic resin with excellent performance. It is a colorless, translucent, thermoplastic, lightweight general-purpose plastic. Polypropylene has chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear processing properties. It has been widely developed and applied in many fields such as machinery, automobiles, electronic appliances, construction, textiles, packaging, agriculture, forestry, fishery and food industry.
[0003] Ordinary polypropylene plastics do not have antibacterial properties and usually require the addition of antibacterial agents. As people pay more and more attention to health and environment, the safety and hygiene of plastic products have become a topic of concern, and antibacterial plastics have emerged. From a microbiological perspective, antibacterial agents focus on inhibiting the growth and reproduction of bacteria during long-term use to maintain a clean and hygienic environment. Generally speaking, the requirements for antibacterial agents are: a. Antibacterial ability and broad-spectrum antibacterial properties; b. Persistence, that is, resistance to washing, wear and tear, and long life; c. Compatibility with the substrate, that is, easy to add to the substrate without reducing product performance.
[0004] Antimicrobial agents can be divided into three types: inorganic, organic and natural biological antimicrobial agents. Different antimicrobial agents have different antimicrobial action mechanisms and effectiveness against the same pathogens, and the same antimicrobial agent has different antimicrobial action mechanisms and inhibition ranges against different pathogens. At present, polypropylene products need to be degraded after use, and the main force of degradation is mainly microorganisms. Organic antimicrobial agents are mainly chemical synthetic substances, and there are still major hidden dangers in their safety. Plastics with added inorganic antimicrobial agents will make it difficult for bacteria to survive and plastic products will be difficult to degrade, which needs to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose an antibacterial and environmentally friendly polypropylene composite plastic and a preparation method thereof.
[0006] An antibacterial and environment-friendly polypropylene composite plastic comprises raw materials including polypropylene, graphene oxide loaded zinc oxide, SBS latex, nano zinc oxide, dispersant, compatibilizer, antioxidant and masterbatch; the mass ratio of polypropylene, graphene oxide loaded zinc oxide, SBS latex, nano zinc oxide, dispersant, compatibilizer, antioxidant and masterbatch is 50-120:5-10:5-15:1-3:2-4:1-2:1-2:1-2; the graphene oxide loaded zinc oxide is obtained by grafting pretreated graphene oxide with zinc oxide deposited on the surface with dendritic polyamide amine; and the pretreated graphene oxide is obtained by adsorbing nano zinc oxide whiskers and loading them on graphene oxide active sheets.
[0007] Preferably, the dispersant is at least one of zinc stearate, polyethylene wax and liquid paraffin.
[0008] Preferably, the compatibilizer is at least one of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride, and methacrylic acid-styrene-butadiene polymer.
[0009] Preferably, the antioxidant is at least one of antioxidant 1010 , antioxidant 168 , and antioxidant 1076 .
[0010] Preferably, the pretreated graphene oxide is prepared by the following specific steps: dispersing nano zinc oxide whiskers in water, adjusting the pH value of the system to 6-6.5, adding graphene oxide and ultrasonically dispersing for 1-2 hours, then adjusting the system to be neutral, standing for 10-20 hours, filtering, washing with water, and drying to obtain the pretreated graphene oxide.
[0011] More preferably, the mass ratio of nano zinc oxide whiskers to graphene oxide is 1-2:1-5.
[0012] More preferably, the frequency of ultrasonic dispersion is 5-10 kHz,
[0013] Preferably, the graphene oxide-supported zinc oxide is prepared by the following specific steps: dissolving zinc nitrate hexahydrate in water, adding hexamethylenetetramine and polyvinyl alcohol and stirring evenly, adding pretreated graphene oxide thereto, stirring at 60-90° C. for 5-10 hours, adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and dendritic polyamidoamine and continuing to stir for 1-4 hours, filtering, washing with water, and drying to obtain graphene oxide-supported zinc oxide.
[0014] The invention disperses nano zinc oxide whiskers in deionized water and adjusts the pH of the system to 6-6.5. The surface of the zinc oxide whiskers carries negative charges and can be effectively adsorbed and loaded on the active sites at the edge of the graphene oxide sheet structure, but the loading amount is low and the binding strength is poor through electrostatic binding.
[0015] The present invention further grows nano zinc oxide on the surface of pretreated graphene oxide, which not only has a very high loading amount but also has a high bonding strength. Since the surface of the obtained product has a large number of active functional groups such as hydroxyl groups and carboxyl groups, dendritic polyamide amine is further grafted on the surface, which can not only form a reinforcing rib structure in polypropylene, effectively enhancing the mechanical strength of the plastic, but also because the graphene oxide loaded zinc oxide is coated in the organic polymer structure, combined with the externally dispersed and bonded nano zinc oxide, it can effectively adjust the antibacterial timeliness, and the antibacterial timeliness is long.
[0016] More preferably, the mass ratio of zinc nitrate hexahydrate, hexamethylenetetramine, polyvinyl alcohol, pretreated graphene oxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and dendritic polyamidoamine is 1-3:2-5:1-3:2-6:0.01-0.1:1-3.
[0017] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0018] S1. Disperse nano zinc oxide, deionized water and dispersant evenly, add SBS latex and continue stirring for 10-20 minutes, and spray dry to obtain zinc oxide-doped SBS;
[0019] S2. Evenly mix polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide, add dispersant, compatibilizer, antioxidant, and masterbatch, and continue stirring for 1-5 minutes to obtain a premix;
[0020] S3, extruding the premix, cooling it in a water tank and air in sequence, and pelletizing it to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0021] Preferably, a twin-screw extruder is used for extrusion in S3, wherein the temperature of zone 1 is set at 150-160°C, the temperature of zone 2 is set at 180-190°C, the temperature of zone 3 is set at 195-205°C, the temperature of zone 4 is set at 200-210°C, the temperature of zone 5 is set at 190-205°C, the head temperature is set at 200-210°C, and the main screw speed is set at 100-300r / min.
[0022] Beneficial effects:
[0023] The present invention adds zinc oxide doped SBS to the polypropylene masterbatch, so that the zinc oxide is better dispersed in the mixed system. After melt blending, not only the masterbatch has a good antibacterial effect, but also the zinc oxide loaded with graphene oxide is dispersed therein, showing high activity, a wide antibacterial spectrum, and stable and long-lasting antibacterial. In addition, the applicant has found through experiments that the present application can promote the degradation of plastics while ensuring excellent antibacterial timeliness, and has no obvious effect on its mechanical properties.
[0024] If nano zinc oxide is directly added to polypropylene plastic, the compatibility is poor. The present invention first disperses nano zinc oxide with SBS latex to enhance the uniformity of the dispersion of nano zinc oxide in polypropylene plastic, so that the polypropylene plastic has good antibacterial performance. In addition, because the graphene oxide loaded zinc oxide is evenly distributed in the polypropylene plastic, rather than just covering the surface of the polypropylene plastic, the polypropylene plastic product still has good antibacterial performance even after being damaged, and has excellent antibacterial performance.
[0025] The present invention adopts a specific process to combine nano zinc oxide into polypropylene plastic, which not only has a long antibacterial effect, but also can effectively solve the problem of difficult degradation, has high mechanical strength, and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The figure is a comparison chart of the mechanical properties of the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3.
[0027] Figure 2 The figure is a comparison chart of the antibacterial effects of the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3 at 0, 3, and 6 months.
[0028] Figure 3 This is a comparison chart of the antibacterial effects of the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3 after one year of exposure.
[0029] Figure 4 This is a comparison chart of the mass loss rate of the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3 after being buried in the soil for one year. DETAILED DESCRIPTION
[0030] The present invention will be further explained below in conjunction with specific embodiments.
[0031] Example 1
[0032] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 50kg of polypropylene, 5kg of graphene oxide loaded zinc oxide, 5kg of SBS latex, 1kg of nano zinc oxide, 2kg of liquid paraffin, 1kg of methacrylic acid-styrene-butadiene polymer, 1kg of antioxidant 1076, and 1kg of masterbatch.
[0033] Graphene oxide supported zinc oxide is prepared by the following specific steps: 1 kg of zinc nitrate hexahydrate is added to 10 kg of deionized water and stirred evenly, 2 kg of hexamethylenetetramine and 1 kg of polyvinyl alcohol are added and stirred evenly, 2 kg of pretreated graphene oxide is added thereto, and the mixture is stirred at a temperature of 60 ° C for 5 h and a stirring speed of 50 r / min, 0.01 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 1 kg of dendritic polyamidoamine are added, and stirring is continued for 1 h, filtered, washed once with deionized water, and dried to obtain graphene oxide supported zinc oxide.
[0034] The pretreated graphene oxide is prepared by the following specific steps: 1 kg of nano zinc oxide whiskers are dispersed in 20 kg of deionized water, the pH value of the system is adjusted to 6-6.5 with 0.1 mol / L hydrochloric acid, 1 kg of graphene oxide is added, ultrasonic dispersion is performed for 1 hour, the ultrasonic frequency is 5 kHz, the system is adjusted to be neutral with 0.1 mol / L sodium hydroxide solution, standing for 10 hours, filtering, washing with deionized water, and drying to obtain the pretreated graphene oxide.
[0035] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0036] S1. Add nano zinc oxide, deionized water and liquid paraffin into a high-speed disperser, disperse at a speed of 1000 r / min for 5 min, add SBS latex and continue stirring for 10 min, and spray dry to obtain zinc oxide-doped SBS;
[0037] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 500 r / min for 10 min, adding liquid paraffin, methacrylic acid-styrene-butadiene polymer, antioxidant 1076, and masterbatch, and continuing stirring for 1 min to obtain a premix;
[0038] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1 is set to 150°C, the temperature of zone 2 is set to 180°C, the temperature of zone 3 is set to 195°C, the temperature of zone 4 is set to 200°C, the temperature of zone 5 is set to 190°C, the temperature of the die head is set to 200°C, the main engine screw speed is set to 100r / min, and the premix is successively cooled by water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0039] Example 2
[0040] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 120kg of polypropylene, 10kg of graphene oxide loaded zinc oxide, 15kg of SBS latex, 3kg of nano zinc oxide, 4kg of liquid paraffin, 2kg of methacrylic acid-styrene-butadiene polymer, 2kg of antioxidant 168, and 2kg of masterbatch.
[0041] Graphene oxide-supported zinc oxide is prepared by the following specific steps: 3 kg of zinc nitrate hexahydrate is added to 30 kg of deionized water and stirred evenly, 5 kg of hexamethylenetetramine and 3 kg of polyvinyl alcohol are added and stirred evenly, 6 kg of pretreated graphene oxide is added thereto, and the mixture is stirred at a temperature of 90 ° C for 10 hours at a stirring speed of 100 r / min, 0.1 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 3 kg of dendritic polyamide amine are added, stirring is continued for 4 hours, filtered, washed 3 times with deionized water, and dried to obtain graphene oxide-supported zinc oxide.
[0042] The pretreated graphene oxide is prepared by the following specific steps: 2 kg of nano zinc oxide whiskers are dispersed in 50 kg of deionized water, the pH value of the system is adjusted to 6-6.5 with 0.2 mol / L hydrochloric acid, 5 kg of graphene oxide is added, ultrasonic dispersion is performed for 2 hours, the ultrasonic frequency is 10 kHz, the system is adjusted to be neutral with 0.2 mol / L sodium hydroxide solution, standing for 20 hours, filtering, washing with deionized water, and drying to obtain the pretreated graphene oxide.
[0043] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0044] S1. Add nano zinc oxide, deionized water and liquid paraffin into a high-speed disperser, disperse at a speed of 5000 r / min for 20 min, add SBS latex and continue stirring for 20 min, and spray dry to obtain zinc oxide-doped SBS;
[0045] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 1500 r / min for 20 min, adding liquid paraffin, methacrylic acid-styrene-butadiene polymer, antioxidant 168, and masterbatch, and continuing stirring for 5 min to obtain a premix;
[0046] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1 is set to 160°C, the temperature of zone 2 is set to 190°C, the temperature of zone 3 is set to 205°C, the temperature of zone 4 is set to 210°C, the temperature of zone 5 is set to 205°C, the temperature of the die head is set to 210°C, the main engine screw speed is set to 300r / min, and the premix is successively cooled by water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0047] Example 3
[0048] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 90kg of polypropylene, 9kg of graphene oxide loaded zinc oxide, 8kg of SBS latex, 2.5kg of nano zinc oxide, 1kg of zinc stearate, 1.5kg of polyethylene wax, 1.7kg of polyethylene grafted maleic anhydride, 1.2kg of antioxidant 1076, and 1.6kg of masterbatch.
[0049] Graphene oxide supported zinc oxide is prepared by the following specific steps: 1.5 kg of zinc nitrate hexahydrate is added to 25 kg of deionized water and stirred evenly, 3 kg of hexamethylenetetramine and 2.5 kg of polyvinyl alcohol are added and stirred evenly, 3 kg of pretreated graphene oxide is added thereto, and the mixture is stirred at a temperature of 80 ° C for 6 h and a stirring speed of 90 r / min, 0.03 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 2.5 kg of dendritic polyamidoamine are added, stirring is continued for 2 h, filtered, washed twice with deionized water, and dried to obtain graphene oxide supported zinc oxide.
[0050] The pretreated graphene oxide was prepared by the following specific steps: 1.7 kg of nano zinc oxide whiskers were dispersed in 30 kg of deionized water, the pH value of the system was adjusted to 6-6.5 with 0.18 mol / L hydrochloric acid, 2 kg of graphene oxide was added, ultrasonic dispersion was performed for 100 min, the ultrasonic frequency was 7 kHz, the system was adjusted to be neutral with 0.18 mol / L sodium hydroxide solution, the system was allowed to stand for 13 h, filtered, washed with deionized water, and dried to obtain the pretreated graphene oxide.
[0051] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0052] S1. Add nano zinc oxide, deionized water and zinc stearate into a high-speed disperser, disperse at a speed of 4000 r / min for 10 min, add SBS latex and continue stirring for 18 min, and spray dry to obtain zinc oxide-doped SBS;
[0053] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 800 r / min for 18 min, adding polyethylene wax, polyethylene grafted maleic anhydride, antioxidant 1076, and masterbatch, and continuing stirring for 2 min to obtain a premix;
[0054] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1, zone 2, zone 3, zone 4, zone 5, and the temperature of zone 1, zone 2, zone 3, zone 4, and zone 5 are set to 158°C, 182°C, 202°C, 204°C, and 200°C, respectively. The head temperature is 202°C, and the main screw speed is 240r / min. The premix is sequentially cooled by a water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0055] Example 4
[0056] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 110kg of polypropylene, 7kg of graphene oxide loaded zinc oxide, 12kg of SBS latex, 1.5kg of nano zinc oxide, 2kg of polyethylene wax, 1.5kg of zinc stearate, 1.3kg of polyethylene grafted maleic anhydride, 1.8kg of antioxidant 1076, and 1.4kg of masterbatch.
[0057] Graphene oxide supported zinc oxide is prepared by the following specific steps: 2.5 kg of zinc nitrate hexahydrate is added to 15 kg of deionized water and stirred evenly, 4 kg of hexamethylenetetramine and 1.5 kg of polyvinyl alcohol are added and stirred evenly, 5 kg of pretreated graphene oxide is added thereto, and the mixture is stirred at a temperature of 70 ° C. for 8 h, and a stirring speed of 70 r / min. 0.07 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 1.5 kg of dendritic polyamidoamine are added, and stirring is continued for 2-3 h. The mixture is filtered, washed twice with deionized water, and dried to obtain graphene oxide supported zinc oxide.
[0058] The pretreated graphene oxide was prepared by the following specific steps: 1.7 kg of nano zinc oxide whiskers were dispersed in 30 kg of deionized water, the pH value of the system was adjusted to 6-6.5 with 0.18 mol / L hydrochloric acid, 2 kg of graphene oxide was added, ultrasonic dispersion was performed for 100 min, the ultrasonic frequency was 7 kHz, the system was adjusted to be neutral with 0.18 mol / L sodium hydroxide solution, the system was allowed to stand for 13 h, filtered, washed with deionized water, and dried to obtain the pretreated graphene oxide.
[0059] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0060] S1. Add nano zinc oxide, deionized water and polyethylene wax into a high-speed disperser, disperse at a speed of 4000 r / min for 10 min, add SBS latex and continue stirring for 12-18 min, and spray dry to obtain zinc oxide-doped SBS;
[0061] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 1200 r / min for 12 min, adding zinc stearate, polyethylene grafted maleic anhydride, antioxidant 1076, and masterbatch, and continuing stirring for 4 min to obtain a premix;
[0062] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1, zone 2, zone 3, zone 4, zone 5, zone 6, zone 7, zone 8, zone 9, zone 10, zone 11, zone 12, zone 13, zone 14, zone 15, zone 16, zone 17, zone 18, zone 19, zone 20, zone 21, zone 22, zone 23, zone 24, zone 25, zone 26, zone 27, zone 28, zone 30, zone 31, zone 32, zone 33, zone 34, zone 35, zone 36, zone 37, zone 38, zone 39, zone 40, zone 41, zone 42, zone 43, zone 44, zone 45, zone 46, zone 47, zone 48, zone 49
[0063] Example 5
[0064] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 100kg of polypropylene, 8kg of graphene oxide loaded zinc oxide, 10kg of SBS latex, 2kg of nano zinc oxide, 3kg of polyethylene wax, 1.5kg of polypropylene grafted maleic anhydride, 1.5kg of antioxidant 1010, and 1.5kg of masterbatch.
[0065] Graphene oxide supported zinc oxide is prepared by the following specific steps: 2 kg of zinc nitrate hexahydrate is added to 20 kg of deionized water and stirred evenly, 3.5 kg of hexamethylenetetramine and 2 kg of polyvinyl alcohol are added and stirred evenly, 4 kg of pretreated graphene oxide is added thereto, and the mixture is stirred at a temperature of 75 ° C. for 7 hours at a stirring speed of 80 r / min, 0.05 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 2 kg of dendritic polyamide amine are added, stirring is continued for 2.5 hours, filtered, washed twice with deionized water, and dried to obtain graphene oxide supported zinc oxide.
[0066] The pretreated graphene oxide is prepared by the following specific steps: 1.5 kg of nano zinc oxide whiskers are dispersed in 35 kg of deionized water, the pH value of the system is adjusted to 6-6.5 with 0.15 mol / L hydrochloric acid, 3 kg of graphene oxide is added, ultrasonic dispersion is performed for 90 minutes, the ultrasonic frequency is 7.5 kHz, the system is adjusted to be neutral with 0.15 mol / L sodium hydroxide solution, standing for 15 hours, filtering, washing with deionized water, and drying to obtain the pretreated graphene oxide.
[0067] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0068] S1. Add nano zinc oxide, deionized water and polyethylene wax into a high-speed disperser, disperse at a speed of 3000 r / min for 13 min, add SBS latex and continue stirring for 15 min, and spray dry to obtain zinc oxide-doped SBS;
[0069] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 1000 r / min for 15 min, adding polyethylene wax, polypropylene grafted maleic anhydride, antioxidant 1010, and masterbatch, and continuing stirring for 3 min to obtain a premix;
[0070] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1 is set to 155°C, the temperature of zone 2 is set to 185°C, the temperature of zone 3 is set to 200°C, the temperature of zone 4 is set to 205°C, the temperature of zone 5 is set to 198°C, the temperature of the die head is set to 205°C, the main engine screw speed is set to 200r / min, and the premix is successively cooled by water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0071] Comparative Example 1
[0072] Commercially available antibacterial polypropylene plastic (purchased from Industrial Product Design (Shanghai) Co., Ltd.).
[0073] Comparative Example 2
[0074] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 100kg of polypropylene, 8kg of graphene oxide loaded zinc oxide, 10kg of SBS latex, 2kg of nano zinc oxide, 3kg of polyethylene wax, 1.5kg of polypropylene grafted maleic anhydride, 1.5kg of antioxidant 1010, and 1.5kg of masterbatch.
[0075] Graphene oxide-supported zinc oxide is prepared by the following specific steps: 2 kg of zinc nitrate hexahydrate is added to 20 kg of deionized water and stirred evenly, 3.5 kg of hexamethylenetetramine and 2 kg of polyvinyl alcohol are added and stirred evenly, 4 kg of pretreated graphene oxide is added thereto, stirred at a temperature of 75 ° C for 7 hours, a stirring speed of 80 r / min, filtered, washed twice with deionized water, and dried to obtain graphene oxide-supported zinc oxide.
[0076] The pretreated graphene oxide is prepared by the following specific steps: 1.5 kg of nano zinc oxide whiskers are dispersed in 35 kg of deionized water, the pH value of the system is adjusted to 6-6.5 with 0.15 mol / L hydrochloric acid, 3 kg of graphene oxide is added, ultrasonic dispersion is performed for 90 minutes, the ultrasonic frequency is 7.5 kHz, the system is adjusted to be neutral with 0.15 mol / L sodium hydroxide solution, standing for 15 hours, filtering, washing with deionized water, and drying to obtain the pretreated graphene oxide.
[0077] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0078] S1. Add nano zinc oxide, deionized water and polyethylene wax into a high-speed disperser, disperse at a speed of 3000 r / min for 13 min, add SBS latex and continue stirring for 15 min, and spray dry to obtain zinc oxide-doped SBS;
[0079] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 1000 r / min for 15 min, adding polyethylene wax, polypropylene grafted maleic anhydride, antioxidant 1010, and masterbatch, and continuing stirring for 3 min to obtain a premix;
[0080] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1 is set to 155°C, the temperature of zone 2 is set to 185°C, the temperature of zone 3 is set to 200°C, the temperature of zone 4 is set to 205°C, the temperature of zone 5 is set to 198°C, the temperature of the die head is set to 205°C, the main engine screw speed is set to 200r / min, and the premix is successively cooled by water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0081] Comparative Example 3
[0082] An antibacterial and environmentally friendly polypropylene composite plastic, whose raw materials include: 100kg of polypropylene, 8kg of graphene oxide loaded zinc oxide, 10kg of SBS latex, 2kg of nano zinc oxide, 3kg of polyethylene wax, 1.5kg of polypropylene grafted maleic anhydride, 1.5kg of antioxidant 1010, and 1.5kg of masterbatch.
[0083] Graphene oxide-supported zinc oxide is prepared by the following specific steps: 4 kg of pretreated graphene oxide is added to 20 kg of deionized water and stirred evenly, stirred at a temperature of 75 ° C for 7 hours, and a stirring speed of 80 r / min, 0.05 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 2 kg of dendritic polyamide amine are added, and stirring is continued for 2.5 hours. Filter, wash twice with deionized water, and dry to obtain graphene oxide-supported zinc oxide.
[0084] The pretreated graphene oxide is prepared by the following specific steps: 1.5 kg of nano zinc oxide whiskers are dispersed in 35 kg of deionized water, the pH value of the system is adjusted to 6-6.5 with 0.15 mol / L hydrochloric acid, 3 kg of graphene oxide is added, ultrasonic dispersion is performed for 90 minutes, the ultrasonic frequency is 7.5 kHz, the system is adjusted to be neutral with 0.15 mol / L sodium hydroxide solution, standing for 15 hours, filtering, washing with deionized water, and drying to obtain the pretreated graphene oxide.
[0085] The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic comprises the following steps:
[0086] S1. Add nano zinc oxide, deionized water and polyethylene wax into a high-speed disperser, disperse at a speed of 3000 r / min for 13 min, add SBS latex and continue stirring for 15 min, and spray dry to obtain zinc oxide-doped SBS;
[0087] S2, adding polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide into a mixer, stirring at a speed of 1000 r / min for 15 min, adding polyethylene wax, polypropylene grafted maleic anhydride, antioxidant 1010, and masterbatch, and continuing stirring for 3 min to obtain a premix;
[0088] S3. The premix is extruded by a twin-screw extruder, wherein the temperature of zone 1 is set to 155°C, the temperature of zone 2 is set to 185°C, the temperature of zone 3 is set to 200°C, the temperature of zone 4 is set to 205°C, the temperature of zone 5 is set to 198°C, the temperature of the die head is set to 205°C, the main engine screw speed is set to 200r / min, and the premix is successively cooled by water tank and air, and pelletized to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
[0089] With reference to GB / T 1040.1-2018 "Determination of Tensile Properties of Plastics Part 1: General Principles" and GB / T 1040.2-2022 "Determination of Tensile Properties of Plastics Part 2: Test Conditions for Molded and Extruded Plastics", the tensile strength test was carried out on the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3, and the sample size was 1A type, and the test speed was 50 mm / min; with reference to GB / T9341-2008 "Determination of Flexural Properties of Plastics", the flexural strength test was carried out on the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3, and the sample size was 80 mm in length, 10 mm in width, and 4 mm in thickness, and the test speed was 5 mm / min; with reference to GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics", the impact strength test was carried out on the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3, and the sample size was A type.
[0090] The results are as follows Figure 1 As shown, the mechanical properties of the antibacterial polypropylene plastic obtained in Example 5 are significantly better than those of the comparative example. However, in Comparative Example 2, no dendritic polyamide amine was used for grafting, and a similar reinforcing rib structure could not be formed in the polypropylene, so that its mechanical strength was similar to that of Comparative Example 1. Although Comparative Example 3 used dendritic polyamide amine for grafting, zinc oxide was not loaded on the surface of the pretreated graphene oxide, so that its reinforcing effect was not as good as that of Example 5.
[0091] The antibacterial effects of the antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3 were tested with reference to GB / T 31402-2015 "Test Method for Antibacterial Performance of Plastic Surfaces", with Escherichia coli (ATCC 8739) and Staphylococcus aureus (ATCC6538P) as test objects. The detection time was immediately after the preparation of each group of antibacterial polypropylene plastics was completed (0 month), and each group of antibacterial polypropylene plastics was placed at room temperature for 3 months and 6 months.
[0092] The results are as follows Figure 2 As shown, the antibacterial rates of the antibacterial polypropylene plastics obtained in Comparative Examples 1 and 3 decrease with the extension of the storage time. However, the antibacterial polypropylene plastics obtained in Example 5 and Comparative Example 2 still have good antibacterial properties after being placed for 6 months, indicating that they both have long-lasting antibacterial properties.
[0093] The antibacterial polypropylene plastics obtained in Example 5 and Comparative Examples 1-3 were injection molded to prepare plastic test pieces with a size of 50 mm in length, 20 mm in width and 1 mm in thickness. After the plastic test pieces were exposed in a cool and ventilated place for 1 year, 75% alcohol was used to disinfect the plastic test pieces. Under a sterile environment, 10 CFU of Staphylococcus aureus, Helicobacter pylori and Candida albicans were implanted in the center of each group of plastic test pieces, respectively, and cultured at 37° C. for 7 days, and the number of colonies was observed and recorded.
[0094] like Figure 3 As shown, the antibacterial polypropylene plastic obtained in Example 5 still has excellent antibacterial effect after being left vacant for one year, which proves that the antibacterial effect of the antibacterial polypropylene plastic obtained in the present invention is long-lasting.
[0095] The antibacterial polypropylene plastic obtained in Example 5 and Comparative Examples 1-3 was injection molded to form a plastic test piece with a size of 50 mm in length, 20 mm in width, and 1 mm in thickness, and air-dried at room temperature. The weight of the plastic test piece was weighed and recorded as the initial weight; it was then buried in soil and stored at a constant temperature of 37°C for 1 year. The plastic test piece was taken out, washed, air-dried at room temperature, and weighed. The weight of the plastic test piece was recorded as the weight after degradation, and the degree of degradation of the plastic test piece was characterized by calculating the mass loss rate.
[0096] like Figure 4 As shown, although the antibacterial polypropylene plastic obtained in Example 5 has a lasting antibacterial effect, the soil environment is more complex, and the content and types of microorganisms are much more than those in a normal environment; in the soil state, the present invention can be quickly decomposed by microorganisms, thereby accelerating the degradation of plastics.
[0097] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An antibacterial and environmentally friendly polypropylene composite plastic, characterized in that: The raw materials include: polypropylene, graphene oxide loaded zinc oxide, SBS latex, nano zinc oxide, dispersant, compatibilizer, antioxidant, masterbatch; the mass ratio of polypropylene, graphene oxide loaded zinc oxide, SBS latex, nano zinc oxide, dispersant, compatibilizer, antioxidant, masterbatch is 50-120: 5-10: 5-15: 1-3: 2-4: 1-2: 1-2: 1-2; The graphene oxide loaded with zinc oxide is obtained by grafting pretreated graphene oxide with zinc oxide deposited on the surface with dendritic polyamide amine; and the pretreated graphene oxide is obtained by adsorbing nano zinc oxide whiskers and loading them on the graphene oxide active sheet. Graphene oxide supported zinc oxide is prepared by the following specific steps: dissolving zinc nitrate hexahydrate in water, adding hexamethylenetetramine and polyvinyl alcohol and stirring evenly, adding pretreated graphene oxide thereto, stirring at 60-90° C. for 5-10 hours, adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and dendritic polyamidoamine and continuing to stir for 1-4 hours, filtering, washing with water, and drying to obtain graphene oxide supported zinc oxide; The pretreated graphene oxide is prepared by the following specific steps: dispersing nano zinc oxide whiskers in water, adjusting the pH value of the system to 6-6.5, adding graphene oxide and ultrasonically dispersing for 1-2 hours, then adjusting the system to be neutral, standing for 10-20 hours, filtering, washing with water, and drying to obtain the pretreated graphene oxide.
2. The antibacterial and environmentally friendly polypropylene composite plastic according to claim 1, characterized in that: The dispersant is at least one of zinc stearate, polyethylene wax and liquid paraffin.
3. The antibacterial and environmentally friendly polypropylene composite plastic according to claim 1, characterized in that: The compatibilizer is at least one of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride, and methacrylic acid-styrene-butadiene polymer.
4. The antibacterial and environmentally friendly polypropylene composite plastic according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
5. The antibacterial and environmentally friendly polypropylene composite plastic according to claim 1, characterized in that: The mass ratio of nano zinc oxide whiskers to graphene oxide is 1-2:1-5.
6. The antibacterial and environmentally friendly polypropylene composite plastic according to claim 1, characterized in that: The mass ratio of zinc nitrate hexahydrate, hexamethylenetetramine, polyvinyl alcohol, pretreated graphene oxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and dendritic polyamidoamine is 1-3:2-5:1-3:2-6:0.01-0.1:1-3.
7. A method for preparing the antibacterial and environmentally friendly polypropylene composite plastic according to any one of claims 1 to 6, characterized in that: The steps include: S1. Disperse nano zinc oxide, deionized water and dispersant evenly, add SBS latex and continue stirring for 10-20 minutes, and spray dry to obtain zinc oxide-doped SBS; S2. Evenly mix polypropylene, zinc oxide-doped SBS, and graphene oxide-loaded zinc oxide, add dispersant, compatibilizer, antioxidant, and masterbatch, and continue stirring for 1-5 minutes to obtain a premix; S3, extruding the premix, cooling it in a water tank and air in sequence, and pelletizing it to obtain an antibacterial and environmentally friendly polypropylene composite plastic.
8. The method for preparing the antibacterial and environmentally friendly polypropylene composite plastic according to claim 7, characterized in that: S3 uses a twin-screw extruder for extrusion, wherein the temperature of zone 1 is set at 150-160°C, the temperature of zone 2 is set at 180-190°C, the temperature of zone 3 is set at 195-205°C, the temperature of zone 4 is set at 200-210°C, the temperature of zone 5 is set at 190-205°C, the temperature of the die head is set at 200-210°C, and the main screw speed is set at 100-300r / min.