A high frequency carbon hydrogen copper clad laminate and preparation method thereof
Through the synergistic effect of modified bismaleimide resin and flame retardants containing Si, P, and B elements, the problems of insufficient dielectric properties and flame retardant properties of traditional copper-clad laminates are solved, and a low dielectric constant, High-frequency hydrocarbon copper-clad laminates with low dielectric loss, good flame retardancy and oxidation resistance improve the performance and safety of electronic products.
Patent Information
- Application Number
- CN202311649736.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-05
AI Technical Summary
Traditional copper-clad laminates have limited dielectric and flame retardant properties in high-frequency circuits, and the preparation process of hydrocarbon resin is complex and flammable, posing safety and environmental risks.
Using 4'-aminomethylbiphenyl-4-phenol and di-p-tolyldichlorosilane to react to generate an intermediate, combined with maleic anhydride to prepare modified bismaleimide resin, and oxidizing octavinyl dichlorosilane Silsesquioxane generates epoxy silsesquioxane, combined with boric acid Form a flame retardant containing Si, P, and B elements, combine hydrocarbon resin, methyl ethyl ketone, toluene, cyanate ester, initiator, flame retardant, antioxidant, and filler to prepare a high-frequency hydrocarbon resin glue, and impregnate it in the electronic On fiberglass cloth and heated and pressed to make copper clad laminate.
It significantly improves the dielectric properties, flame retardant properties and oxidation resistance of the copper-clad laminate, reduces the dielectric constant and dielectric loss, extends the service life, and improves the performance and reliability of electronic products.
Smart Images

Figure BDA0004586991200000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminates, in particular to a high-frequency carbon-hydrogen copper clad laminate and a preparation method thereof. Background Art
[0002] With the continuous development of electronic communication technology, the demand for high-frequency circuits is increasing. Hydrocarbon resin is a commonly used copper clad laminate material with good conductivity and high-frequency characteristics, so it is widely used in high-frequency circuits.
[0003] Traditional copper clad laminates usually use epoxy resin as the substrate, but their high-frequency performance and flame retardant properties are limited. Compared with traditional copper clad laminates, hydrocarbon copper clad laminates have lower dielectric constants and loss factors, which can effectively reduce energy loss during signal transmission and improve the stability and reliability of signal transmission. However, due to the special properties of hydrocarbon resins, the preparation process is relatively complicated, and the content and uniformity of the resin need to be controlled to ensure the stable performance of the copper clad laminate. At the same time, hydrocarbon resins have poor flame retardant properties. When exposed to heat sources or flames, they are easy to burn and release toxic gases and smoke, posing potential risks to personal safety and the environment.
[0004] Therefore, we propose a high-frequency carbon-hydrogen copper clad laminate and a preparation method thereof. Summary of the invention
[0005] The object of the present invention is to provide a high-frequency carbon-hydrogen copper-clad laminate and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a high-frequency carbon-hydrogen copper-clad laminate comprises the following steps:
[0008] S1: 4'-aminomethylbiphenyl-4-phenol and triethylamine are mixed evenly, butanone is added and mixed, the temperature is raised to 60-70°C, di-p-tolyldichlorosilane is added dropwise, the dripping is completed in 1-2 hours, the temperature is raised to 75-85°C, reflux reaction is carried out for 10-12 hours, and the intermediate is obtained by filtering, washing and recrystallization; the intermediate, maleic anhydride and toluene are mixed evenly, reacted at room temperature for 6-8 hours, and modified bismaleimide resin is obtained by vacuum distillation and multiple purification;
[0009] S2: Evenly mix hydrocarbon resin and modified bismaleimide resin, raise the temperature to 50-70°C, add butanone, toluene, cyanate ester, initiator, flame retardant, antioxidant and filler, and evenly mix to obtain high-frequency hydrocarbon resin glue;
[0010] S3: dipping the electronic glass fiber cloth in high-frequency hydrocarbon resin glue for dipping treatment, taking it out, and baking it at 140-160° C. for 5-10 minutes to obtain a prepreg;
[0011] S4: Overlap 4 to 8 prepreg sheets to obtain overlapping sheets, place a copper foil on the upper surface and the lower surface of the overlapping sheets, heat and pressurize, and cool to room temperature to obtain a copper clad laminate.
[0012] Furthermore, the mass ratio of 4'-aminomethylbiphenyl-4-phenol to triethylamine in S1 is 1:(0.5-0.6).
[0013] Furthermore, the mass of butanone in S1 is 1-2 times the mass of 4'-aminomethylbiphenyl-4-phenol.
[0014] Furthermore, the mass of the di-p-tolyldichlorosilane in S1 is 0.7-0.8 times the mass of 4'-aminomethylbiphenyl-4-phenol.
[0015] Furthermore, the mass ratio of the intermediate, maleic anhydride and toluene in S1 is 1:(0.25-0.30):(1.0-1.5).
[0016] Furthermore, the S2 medium-high frequency hydrocarbon resin glue includes the following components by weight: 80-100 parts of hydrocarbon resin, 30-50 parts of modified bismaleimide resin, 20-30 parts of butanone, 80-100 parts of toluene, 20-40 parts of cyanate ester, 2-6 parts of initiator, 15-30 parts of flame retardant, 0.1-5 parts of antioxidant, and 20-40 parts of filler.
[0017] Furthermore, the hydrocarbon resin is composed of 50-60 parts by mass of 1,2-polybutadiene and 30-40 parts by mass of hydrogenated styrene-butadiene block copolymer.
[0018] Furthermore, the molecular weight of the 1,2-polybutadiene is 2000-7000, the molecular weight of the hydrogenated styrene-butadiene block copolymer is 20000-250000, the styrene content is 10-40%, the toluene solution viscosity is 200-5000 mpas, the hardness is 70-88, and the degree of hydrogenation is ≥97%.
[0019] Furthermore, the cyanate ester is a bisphenol M type cyanate ester monomer.
[0020] Furthermore, the initiator is composed of 1-2 parts by mass of 1,3-dibutylperoxyisopropylbenzene and 1-4 parts by mass of di-tert-butyl peroxide.
[0021] Furthermore, the preparation method of the flame retardant is as follows:
[0022] Step (1): octavinyl silsesquioxane and tetrahydrofuran are uniformly mixed, a mixed solution of m-chloroperbenzoic acid and dichloromethane is added, the mixture is stirred uniformly, the temperature is raised to 40-50° C., condensed and refluxed for 46-48 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane;
[0023] Step (2): Under nitrogen protection, epoxy silsesquioxane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene are mixed evenly, the temperature is raised to 75-85° C., azobisisobutyronitrile is added and mixed evenly, the mixture is kept warm for reaction for 10-12 hours, the temperature is lowered to 40-50° C., boric acid solution is added dropwise for 1-2 hours, the mixture is reacted for 1-2 hours, the mixture is cooled to room temperature, filtered, washed and dried to obtain a flame retardant.
[0024] In the above technical scheme, epoxy silsesquioxane can be generated by oxidizing octavinyl silsesquioxane; the PH bond of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide can react with the epoxy group in epoxy silsesquioxane to generate -OH group and introduce P element; then, boric acid is added to the reaction system to react with the -OH group and introduce B element to obtain a flame retardant having excellent flame retardant effect.
[0025] Furthermore, in the step (1), the mass ratio of octavinylsilsesquioxane to tetrahydrofuran is 1:(10-12).
[0026] Furthermore, in the step (1), the mass ratio of m-chloroperbenzoic acid to dichloromethane is 1:(3-4), and the mass of m-chloroperbenzoic acid is 2.5-3.0 times the mass of octavinylsilsesquioxane.
[0027] Furthermore, in the step (2), the mass ratio of epoxysilsesquioxane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene is 1:(3.0-3.2):(4-5).
[0028] Furthermore, in the step (2), the mass of azobisisobutyronitrile is 0.5-1.5% of the total mass of epoxysilsesquioxane and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0029] Furthermore, in step (2), the concentration of the boric acid solution is 4-5 wt %, and the amount used is 50-60% of the mass of the epoxy silsesquioxane.
[0030] Furthermore, the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.
[0031] Furthermore, the filler is composed of 10-20 parts by mass of fused silicon powder and 10-20 parts by mass of zirconium dioxide.
[0032] Furthermore, the process conditions of the dipping treatment in S3 are: temperature 25-50° C., time 5-15 min, and a mass ratio of high-frequency hydrocarbon resin glue to electronic glass fiber cloth of 1:(5-10).
[0033] Furthermore, the heating and pressurizing process conditions in S4 are: temperature 190-220° C., pressure 2-6 MPa, and time 2-4 h.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. A high-frequency carbon-hydrogen copper-clad laminate and a preparation method thereof of the present invention, wherein the hydroxyl group of 4'-aminomethylbiphenyl-4-phenol and the chlorine group of di-p-tolyldichlorosilane are reacted to introduce a siloxane structure with high bond energy and good flexibility to obtain an intermediate, and maleic anhydride is reacted with the -NH2 bond in the intermediate to obtain a modified bismaleimide. By combining maleimide with an organic silane structure, not only the formability and toughness of the material can be improved, but also the dielectric constant, dielectric loss and thermal expansion coefficient of the maleimide resin are reduced, thereby improving the dielectric properties of the material.
[0036] 2. A high-frequency carbon-hydrogen copper-clad laminate and a preparation method thereof of the present invention can generate epoxy silsesquioxane by oxidizing octavinyl silsesquioxane; the PH bond of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide can react with the epoxy group in epoxy silsesquioxane to generate -OH group and introduce P element; then, boric acid is added to the reaction system to react with -OH group and introduce B element to obtain a flame retardant containing Si, P and B elements, which has excellent flame retardant properties. Through the synergistic flame retardant effect of these elements, the flame retardant properties of the material are significantly improved, wherein the Si element can play a flame retardant effect by generating a silicon-carbon barrier layer during combustion; the P element can play a flame retardant role by forming compounds such as phosphophosphates to hinder heat conduction and gas phase combustion reaction during combustion; the B element can absorb heat during combustion by forming compounds such as boron oxides, reduce combustion temperature, and slow down combustion rate, thereby improving the flame retardant properties of the material. At the same time, the flame retardant has a cage-like highly symmetrical siloxane structure, with a low dielectric constant and dielectric loss, which can not only improve the flame retardant properties of the copper clad laminate, but also give it excellent dielectric properties.
[0037] 3. A high-frequency carbon-hydrogen copper-clad laminate and a preparation method thereof of the present invention, wherein a carbon-hydrogen resin and a modified bismaleimide resin are uniformly mixed, and combined with butanone, toluene, cyanate ester, initiator, flame retardant, antioxidant, and filler, the obtained high-frequency carbon-hydrogen resin glue has good adhesion, dielectric properties, flame retardancy, and oxidation resistance. Using the preparation method of the high-frequency carbon-hydrogen copper-clad laminate of the present invention, a copper-clad laminate with low dielectric constant, low dielectric loss, good flame retardancy, and oxidation resistance can be obtained, thereby extending its service life and improving the performance and reliability of electronic products. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] In this embodiment, 1,2-polybutadiene: molecular weight 2000-7000 Shanghai McLean Biochemical Technology Co., Ltd.; hydrogenated styrene-butadiene block copolymer: American Kraton FG1901, molecular weight 20000-250000, styrene content 10-40%, toluene solution viscosity 200-5000mpas, hardness 70-88, hydrogenation degree ≥97%, from Shanghai Furun Plastic Technology Co., Ltd.; bisphenol M type cyanate monomer: content 98.5%, from Hubei Jiahui Xingcheng Biotechnology Co., Ltd.; fused silicon powder: 400-600 mesh, from Donghai County Jingjing Silicon Product Processing Plant; zirconium dioxide: 30-100nm, from Jiangsu Tianxing New Materials Co., Ltd.; electronic glass fiber cloth: 2116 type, from Hejian Zhongchi Jiaye Insulation Materials Co., Ltd.; copper foil: T2 copper, thickness 6μm, from Wenzhou Hongfeng Electrical Alloy Co., Ltd.
[0040] In the following examples and comparative examples, 1 part is equal to 10 g.
[0041] Embodiment 1: A method for preparing a high-frequency carbon-hydrogen copper-clad laminate, comprising the following processes:
[0042] S1: 30 parts of 4'-aminomethylbiphenyl-4-phenol and 15 parts of triethylamine were mixed evenly, 30 parts of butanone were added and mixed, the temperature was raised to 60°C, 21 parts of di-p-tolyldichlorosilane were added dropwise, the temperature was raised to 75°C, refluxed for 10 hours, filtered, washed and recrystallized to obtain an intermediate; 30 parts of the intermediate, 7.5 parts of maleic anhydride and 30 parts of toluene were mixed evenly, reacted at room temperature for 6 hours, and subjected to reduced pressure distillation and multiple purifications to obtain a modified bismaleimide resin;
[0043] S2: 50 parts of 1,2-polybutadiene, 30 parts of hydrogenated styrene-butadiene block copolymer and 30 parts of modified bismaleimide resin are mixed evenly, the temperature is raised to 50° C., 20 parts of butanone, 80 parts of toluene, 20 parts of bisphenol M type cyanate monomer, 1 part of 1,3-dibutyl peroxyisopropylbenzene, 1 part of di-tert-butyl peroxide, 15 parts of flame retardant, 0.1 part of tris(2,4-di-tert-butylphenyl) phosphite, 10 parts of fused silica powder and 10 parts of zirconium dioxide are added and mixed evenly to obtain a high-frequency hydrocarbon resin glue;
[0044] S3: The electronic glass fiber cloth is immersed in a high-frequency hydrocarbon resin glue solution for dipping treatment (temperature 25°C, time 5 minutes, the mass ratio of the high-frequency hydrocarbon resin glue solution to the electronic glass fiber cloth is 1:5), taken out, and baked at 140°C for 10 minutes to obtain a semi-cured sheet;
[0045] S4: overlapping four prepregs to obtain overlapping sheets, placing a copper foil on the upper and lower surfaces of the overlapping sheets, heating and pressurizing at a temperature of 190° C., a pressure of 2 MPa, and a time of 2 h, and cooling to room temperature to obtain a copper clad laminate;
[0046] The preparation process of the flame retardant is as follows:
[0047] Step (1): 5 parts of octavinyl silsesquioxane and 50 parts of tetrahydrofuran are mixed uniformly, and a mixed solution of 7.5 parts of m-chloroperbenzoic acid and 22.5 parts of dichloromethane is added, and the mixture is stirred uniformly, heated to 40° C., condensed and refluxed for 46 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane;
[0048] Step (2): Under nitrogen protection, 5 parts of epoxy silsesquioxane, 15 parts of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 20 parts of toluene are mixed evenly, the temperature is raised to 75° C., 0.1 parts of azobisisobutyronitrile are added and mixed evenly, the mixture is kept warm for reaction for 10 hours, the temperature is lowered to 40° C., 2.5 parts of 4 wt% boric acid solution are added dropwise, the mixture is dripped over a period of 1 hour, the mixture is reacted for 1 hour, the mixture is cooled to room temperature, filtered, washed and dried to obtain a flame retardant.
[0049] Embodiment 2: A method for preparing a high-frequency carbon-hydrogen copper-clad laminate, comprising the following processes:
[0050] S1: 40 parts of 4'-aminomethylbiphenyl-4-phenol and 22 parts of triethylamine were mixed evenly, 60 parts of butanone were added, the mixture was heated to 65°C, 30 parts of di-p-tolyldichlorosilane were added dropwise, the dripping was completed in 1.5 hours, the mixture was heated to 80°C, refluxed for 11 hours, filtered, washed, and recrystallized to obtain an intermediate; 40 parts of the intermediate, 11 parts of maleic anhydride and 50 parts of toluene were mixed evenly, reacted at room temperature for 7 hours, and the modified bismaleimide resin was obtained by vacuum distillation and multiple purifications;
[0051] S2: 55 parts of 1,2-polybutadiene, 35 parts of hydrogenated styrene-butadiene block copolymer and 40 parts of modified bismaleimide resin are mixed evenly, the temperature is raised to 60°C, 25 parts of butanone, 90 parts of toluene, 30 parts of bisphenol M type cyanate monomer, 1.5 parts of 1,3-dibutyl peroxyisopropylbenzene, 2 parts of di-tert-butyl peroxide, 20 parts of flame retardant, 3 parts of tris(2,4-di-tert-butylphenyl) phosphite, 15 parts of fused silica powder and 15 parts of zirconium dioxide are added and mixed evenly to obtain a high-frequency hydrocarbon resin glue;
[0052] S3: The electronic glass fiber cloth is immersed in a high-frequency hydrocarbon resin glue solution for dipping treatment (temperature 40°C, time 10 minutes, the mass ratio of the high-frequency hydrocarbon resin glue solution to the electronic glass fiber cloth is 1:8), taken out, and baked at 150°C for 8 minutes to obtain a semi-cured sheet;
[0053] S4: overlapping 6 prepregs to obtain overlapping sheets, placing a copper foil on the upper and lower surfaces of the overlapping sheets, heating and pressurizing at a temperature of 200° C., a pressure of 4 MPa, and a time of 3 h, and cooling to room temperature to obtain a copper clad laminate;
[0054] The preparation process of the flame retardant is as follows:
[0055] Step (1): 7 parts of octavinyl silsesquioxane and 77 parts of tetrahydrofuran are mixed uniformly, and a mixed solution of 20 parts of m-chloroperbenzoic acid and 70 parts of dichloromethane is added, and the mixture is stirred uniformly, heated to 45° C., condensed and refluxed for 47 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane;
[0056] Step (2): Under nitrogen protection, 6.5 parts of epoxy silsesquioxane, 20 parts of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 30 parts of toluene are mixed evenly, the temperature is raised to 80° C., 0.27 parts of azobisisobutyronitrile are added and mixed evenly, the mixture is kept warm for reaction for 11 hours, the temperature is lowered to 45° C., 3.6 parts of 4.5wt% boric acid solution are added dropwise, the mixture is dripped over a period of 1.5 hours, the mixture is reacted for 1.5 hours, the mixture is cooled to room temperature, filtered, washed and dried to obtain a flame retardant.
[0057] Embodiment 3: A method for preparing a high-frequency carbon-hydrogen copper-clad laminate, comprising the following process:
[0058] S1: 50 parts of 4'-aminomethylbiphenyl-4-phenol and 30 parts of triethylamine were mixed evenly, 100 parts of butanone were added and mixed, the temperature was raised to 70°C, 40 parts of di-p-tolyldichlorosilane were added dropwise, the dripping was completed in 2 hours, the temperature was raised to 85°C, refluxed for 12 hours, filtered, washed and recrystallized to obtain an intermediate; 50 parts of the intermediate, 15 parts of maleic anhydride and 75 parts of toluene were mixed evenly, reacted at room temperature for 8 hours, and the modified bismaleimide resin was obtained by vacuum distillation and multiple purifications;
[0059] S2: 60 parts of 1,2-polybutadiene, 40 parts of hydrogenated styrene-butadiene block copolymer and 50 parts of modified bismaleimide resin are mixed evenly, the temperature is raised to 70°C, 30 parts of butanone, 100 parts of toluene, 40 parts of bisphenol M type cyanate monomer, 2 parts of 1,3-dibutyl peroxyisopropylbenzene, 4 parts of di-tert-butyl peroxide, 30 parts of flame retardant, 5 parts of tris(2,4-di-tert-butylphenyl) phosphite, 20 parts of fused silica powder and 20 parts of zirconium dioxide are added and mixed evenly to obtain a high-frequency hydrocarbon resin glue;
[0060] S3: The electronic glass fiber cloth is immersed in a high-frequency hydrocarbon resin glue solution for dipping treatment (temperature 50°C, time 15 minutes, the mass ratio of the high-frequency hydrocarbon resin glue solution to the electronic glass fiber cloth is 1:10), taken out, and baked at 160°C for 5 minutes to obtain a semi-cured sheet;
[0061] S4: 8 prepregs are overlapped to obtain an overlapped sheet, a copper foil is placed on the upper surface and the lower surface of the overlapped sheet, and the overlapped sheet is heated and pressurized at a temperature of 220° C. and a pressure of 6 MPa for 4 h, and then cooled to room temperature to obtain a copper clad laminate;
[0062] The preparation process of the flame retardant is as follows:
[0063] Step (1): 10 parts of octavinyl silsesquioxane and 120 parts of tetrahydrofuran are mixed uniformly, 30 parts of a mixed solution of m-chloroperbenzoic acid and 120 parts of dichloromethane are added, the mixture is stirred uniformly, the temperature is raised to 50° C., condensed and refluxed for 48 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane;
[0064] Step (2): Under nitrogen protection, 10 parts of epoxy silsesquioxane, 32 parts of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 50 parts of toluene are mixed evenly, the temperature is raised to 85° C., 0.63 parts of azobisisobutyronitrile are added and mixed evenly, the mixture is kept warm for reaction for 12 hours, the temperature is lowered to 50° C., 6 parts of 5wt% boric acid solution are added dropwise, the mixture is dripped over a period of 2 hours, the mixture is reacted for 2 hours, the mixture is cooled to room temperature, filtered, washed and dried to obtain a flame retardant.
[0065] Comparative Example 1: The S2 medium-high frequency hydrocarbon resin glue includes the following components by weight: 50 parts of 1,2-polybutadiene, 30 parts of hydrogenated styrene-butadiene block copolymer, 30 parts of bismaleimide resin, 20 parts of butanone, 80 parts of toluene, 20 parts of bisphenol M type cyanate monomer, 1 part of 1,3-dibutylperoxyisopropylbenzene, 1 part of di-tert-butyl peroxide, 15 parts of flame retardant, 0.1 part of tris(2,4-di-tert-butylphenyl) phosphite, 10 parts of molten silica powder, and 10 parts of zirconium dioxide; compared with Example 1, Comparative Example 1 replaces the modified bismaleimide resin with ordinary bismaleimide resin (sourced from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.), and the remaining steps and processes are the same as Example 1.
[0066] Comparative Example 2: The high-frequency hydrocarbon resin glue in S2 includes the following components by weight: 50 parts of 1,2-polybutadiene, 30 parts of hydrogenated styrene-butadiene block copolymer, 30 parts of modified bismaleimide resin, 20 parts of butanone, 80 parts of toluene, 20 parts of bisphenol M type cyanate monomer, 1 part of 1,3-dibutylperoxyisopropylbenzene, 1 part of di-tert-butyl peroxide, 15 parts of decabromodiphenylethane, 0.1 part of tris(2,4-di-tert-butylphenyl) phosphite, 10 parts of fused silica powder, and 10 parts of zirconium dioxide; compared with Example 1, Comparative Example 2 does not include the preparation process of the flame retardant, and the flame retardant in S2 is replaced by decabromodiphenylethane; the remaining steps and processes are the same as those in Example 1.
[0067] Comparative Example 3: The S2 medium-high frequency hydrocarbon resin glue includes the following components by weight: 50 parts of 1,2-polybutadiene, 30 parts of hydrogenated styrene-butadiene block copolymer, 5 parts of modified bismaleimide resin, 20 parts of butanone, 80 parts of toluene, 20 parts of bisphenol M type cyanate monomer, 1 part of 1,3-dibutylperoxyisopropylbenzene, 1 part of di-tert-butyl peroxide, 15 parts of flame retardant, 0.1 part of tris(2,4-di-tert-butylphenyl) phosphite, 10 parts of molten silica powder, and 10 parts of zirconium dioxide; compared with Example 1, Comparative Example 3 adds 5 parts of modified bismaleimide resin, and the preparation process of the flame retardant is deleted. The remaining steps and processes are the same as Example 2.
[0068] Comparative Example 4: A method for preparing a high-frequency carbon-hydrogen copper-clad laminate, comprising the following processes:
[0069] The preparation process of the flame retardant is as follows:
[0070] Step (1): 7 parts of octavinyl silsesquioxane and 77 parts of tetrahydrofuran are mixed uniformly, and a mixed solution of 20 parts of m-chloroperbenzoic acid and 70 parts of dichloromethane is added, and the mixture is stirred uniformly, heated to 45° C., condensed and refluxed for 47 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane;
[0071] Step (2): Under nitrogen protection, 6.5 parts of epoxy silsesquioxane, 6.5 parts of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 6.5 parts of toluene are mixed evenly, the temperature is raised to 80° C., 0.27 parts of azobisisobutyronitrile are added and mixed evenly, the mixture is kept warm for reaction for 11 hours, the temperature is lowered to 45° C., 3.6 parts of 4.5wt% boric acid solution are added dropwise, the mixture is dripped over a period of 1.5 hours, the mixture is reacted for 1.5 hours, the mixture is cooled to room temperature, filtered, washed and dried to obtain a flame retardant.
[0072] Compared with Example 2, in step (2) of Comparative Example 4, the mass ratio of epoxysilsesquioxane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene is 1:1:1, and the remaining steps are the same as Example 2.
[0073] experiment
[0074] The copper-clad laminates obtained in Examples 1-3 and Comparative Examples 1-4 were taken to prepare samples, and their properties were tested and the test results were recorded:
[0075] The dielectric constant and dielectric loss factor were determined according to the IPC-TM650-2.5.5.9 standard. The experimental steps were as follows: the copper clad laminate sample was cut into a size of 50 mm × 50 mm, and measured using a SPDR (split dielectric resonator) at a test frequency of 10 GHz. The test instrument was started and the data was recorded.
[0076] The flame retardancy is determined according to the vertical combustion method of the US UL-94 standard. The experimental steps are as follows: cut the copper clad laminate sample into a size of 100mm×10mm, place it vertically on the fixture of the combustion device, ensure that the lower end of the sample is about 20mm away from the flame source, use the flame source to ignite the lower end of the sample, and observe the combustion characteristics of the sample, including burning time, dripping, flame spread, etc. According to the combustion characteristics of the sample, it is divided into the following grades: V-0 grade: the burning time of the sample does not exceed 10 seconds, no sparks or burning drips are generated after the flame is extinguished, and the burning diffusion distance of the upper part of the sample does not exceed 50mm; V-1 grade: the burning time of the sample does not exceed 30 seconds, no sparks or burning drips are generated after the flame is extinguished, and the burning diffusion distance of the upper part of the sample does not exceed 75mm; V-2 grade: the burning time of the sample does not exceed 30 seconds, no sparks or burning drips are generated after the flame is extinguished, and the burning diffusion distance of the upper part of the sample does not exceed 125mm.
[0077] Test Results
[0078]
[0079] According to the data in the above table, we can clearly draw the following conclusions:
[0080] 1. Compared with Comparative Example 1, the dielectric constant and dielectric loss of the products obtained in Examples 1-3 are reduced, indicating that compared with ordinary bismaleimide resins, the modified bismaleimide resin prepared by the present invention can significantly improve the dielectric properties of copper clad laminates.
[0081] 2. Compared with Examples 1-3, the flame retardancy of the product obtained in Comparative Example 2 is reduced. It can be seen that compared with decabromodiphenylethane, the flame retardant prepared by the present invention has a better flame retardant effect.
[0082] 3. Compared with Examples 1-3, the dielectric properties of the product obtained in Comparative Example 3 are reduced, and it can be seen that adding the modified bismaleimide resin ratio within the range described in the present invention can improve the dielectric properties of the copper clad laminate; the flame retardant properties of the product described in Comparative Example 4 are reduced, indicating that the flame retardant of the present invention is affected by the ratio of each reagent in its preparation process. Selecting the reagent ratio within the range can improve the flame retardant properties of the flame retardant, thereby extending the service life of the copper clad laminate.
[0083] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-frequency carbon-hydrogen copper-clad laminate. Features: The following steps are involved: S1: 4'-aminomethylbiphenyl-4-phenol and triethylamine are mixed evenly, butanone is added and mixed, the temperature is raised to 60-70°C, di-p-tolyldichlorosilane is added dropwise, the dripping is completed in 1-2 hours, the temperature is raised to 75-85°C, reflux reaction is carried out for 10-12 hours, and the intermediate is obtained by filtering, washing and recrystallization; the intermediate, maleic anhydride and toluene are mixed evenly, reacted at room temperature for 6-8 hours, and modified bismaleimide resin is obtained by vacuum distillation and multiple purification; S2: Evenly mix hydrocarbon resin and modified bismaleimide resin, raise the temperature to 50-70°C, add butanone, toluene, cyanate ester, initiator, flame retardant, antioxidant and filler, and evenly mix to obtain high-frequency hydrocarbon resin glue; S3: dipping the electronic glass fiber cloth in high-frequency hydrocarbon resin glue for dipping treatment, taking it out, and baking it at 140-160° C. for 5-10 minutes to obtain a prepreg; S4: overlapping 4 to 8 prepregs to obtain overlapping sheets, placing a copper foil on the upper surface and the lower surface of the overlapping sheets, heating and pressurizing, and cooling to room temperature to obtain a copper clad laminate; The S2 high frequency hydrocarbon resin glue comprises the following components by weight: 80-100 parts of hydrocarbon resin, 30-50 parts of modified bismaleimide resin, 20-30 parts of butanone, 80-100 parts of toluene, 20-40 parts of cyanate ester, 2-6 parts of initiator, 15-30 parts of flame retardant, 0.1-5 parts of antioxidant, and 20-40 parts of filler; The preparation process of the flame retardant is as follows: Step (1): octavinyl silsesquioxane and tetrahydrofuran are uniformly mixed, a mixed solution of m-chloroperbenzoic acid and dichloromethane is added, the mixture is stirred uniformly, the temperature is raised to 40-50° C., condensed and refluxed for 46-48 hours, cooled in an ice bath, filtered, washed multiple times, and evaporated by rotary evaporation to obtain epoxy silsesquioxane; Step (2): under nitrogen protection, epoxy silsesquioxane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene are mixed evenly, the temperature is raised to 75-85° C., azobisisobutyronitrile is added and mixed evenly, the temperature is kept to react for 10-12 hours, the temperature is lowered to 40-50° C., boric acid solution is added dropwise, the dripping is completed within 1-2 hours, the reaction is carried out for 1-2 hours, the flame retardant is obtained after cooling to room temperature, filtering, washing and drying; In the step (2), the mass ratio of epoxysilsesquioxane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene is 1:(3.0-3.2):(4-5).
2. A method for preparing a high-frequency carbon-hydrogen copper-clad laminate according to claim 1, Features: The mass of the di-p-tolyldichlorosilane in S1 is 0.7-0.8 times the mass of 4'-aminomethylbiphenyl-4-phenol.
3. A method for preparing a high-frequency carbon-hydrogen copper-clad laminate according to claim 1, Features: The hydrocarbon resin is composed of 50-60 parts by weight of 1,2-polybutadiene and 30-40 parts by weight of hydrogenated styrene-butadiene block copolymer.
4. The method for preparing a high-frequency carbon-hydrogen copper-clad laminate according to claim 1, Features: The initiator is composed of 1-2 parts by mass of 1,3-dibutylperoxyisopropylbenzene and 1-4 parts by mass of di-tert-butyl peroxide.
5. The method for preparing a high-frequency carbon-hydrogen copper-clad laminate according to claim 1, Features: In the step (1), the mass ratio of chloroperbenzoic acid to dichloromethane is 1:(3-4), and the mass of m-chloroperbenzoic acid is 2.5-3.0 times the mass of octavinylsilsesquioxane.
6. The method for preparing a high-frequency carbon-hydrogen copper-clad laminate according to claim 1, Features: The heating and pressurizing process conditions in S4 are: temperature 190-220° C., pressure 2-6 MPa, and time 2-4 h.
7. A high-frequency carbon-hydrogen copper-clad laminate prepared according to the preparation method according to any one of claims 1 to 6.