A method for preparing silver powder
Silver powder is prepared by reacting silver nitrate with copper powder through ultrasonic oscillation, which solves the problems of complex processes and wastewater pollution in the existing technology, and realizes efficient and environmentally friendly preparation of silver powder, and is suitable for applications in various electronic fields.
Patent Information
- Application Number
- CN202311359380.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-10-18
AI Technical Summary
The existing silver powder synthesis process is complex and produces a large amount of wastewater, requiring high temperature conditions, resulting in environmental pollution and low production efficiency.
Ultrasonic oscillation method is used to mix silver nitrate with copper powder to prepare silver powder to avoid high temperature conditions and reduce waste liquid generation. Ethanol is used as a morphological regulator to control the shape of the particles.
It realizes efficient preparation of silver powder, small particle size, good uniformity, fast speed, and does not produce organic waste liquid. It is suitable for applications in various electronic fields.
Smart Images

Figure CN117620193B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive materials, and in particular to a method for preparing silver powder. Background Art
[0002] Silver micro-nano powder is a key material for solving the current power semiconductor packaging and advanced integrated circuit heat dissipation. It can be used as sintered silver paste, conductive silver glue, nano solder bonding material, electromagnetic shielding material, etc., and has a wide range of applications in new energy vehicles, radio frequency communications, smart grids, wind power, photovoltaics, optoelectronics and other fields. However, the current synthesis of silver powder is relatively cumbersome. Usually, organic solvents are used to react with silver nitrate at high temperature to obtain silver powder, and then a large amount of organic matter is removed by water washing. On the one hand, the process is complicated, and on the other hand, a large amount of wastewater is generated.
[0003] Therefore, there is an urgent need to develop an environmentally friendly, efficient and controllable method for preparing silver powder. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing silver powder. The method does not require high temperature conditions and does not generate organic waste liquid.
[0005] According to a first aspect of the present invention, a method for preparing silver powder is provided, comprising the following steps:
[0006] S1. Ultrasonic vibration is applied to the saturated silver nitrate solution;
[0007] S2. Under ultrasonic conditions, copper powder and saturated silver nitrate solution are mixed for reaction, and then centrifuged to obtain silver powder.
[0008] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:
[0009] The invention adopts silver nitrate as a silver source and copper powder as a reducing agent, and performs a reaction under ultrasonic conditions to prepare silver powder. The reaction does not need to be performed under high temperature conditions and does not generate a large amount of waste liquid. The prepared silver powder particles have a small size and good uniformity. Unlike silver nanoparticles, it does not need to be synthesized at high temperature and needs to be cleaned, and the preparation speed is fast.
[0010] According to some embodiments of the present invention, the power of the ultrasound is 100-300 W. Therefore, within the above ultrasound power range, the size of the silver powder is small.
[0011] According to some embodiments of the present invention, the ultrasonic time is 3 to 5 minutes. Therefore, within the above ultrasonic time range, the size of the silver powder is more uniform.
[0012] According to some embodiments of the present invention, the mass ratio of the silver nitrate to the copper powder is (2.5-20):1.
[0013] According to some embodiments of the present invention, the particle size of the copper powder is 10-100000 nm. Therefore, any value within the range of 10-100000 nm is acceptable, or a range consisting of any two of the above values.
[0014] According to some embodiments of the present invention, the centrifugal rotation speed is 1000-7000 rpm.
[0015] According to some embodiments of the present invention, the centrifugation time is 3 to 10 minutes.
[0016] According to some embodiments of the present invention, step S1 further comprises mixing an ethanol solution with a saturated silver nitrate solution, so that when ethanol is introduced into the reaction, the ethanol acts as a morphology regulator to prepare flaky silver powder.
[0017] According to some embodiments of the present invention, the ethanol accounts for 20% to 80% of the total.
[0018] According to some embodiments of the present invention, the volume fraction of the ethanol solution is 30-50%.
[0019] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0021] Figure 1 is a SEM image of the silver powder prepared in Example 1 of the present invention;
[0022] Figure 2 is a SEM image of the silver powder prepared in Example 2 of the present invention;
[0023] Figure 3 is a SEM image of the silver powder prepared in Example 3 of the present invention;
[0024] Figure 4 is a SEM image of the silver powder prepared in Example 4 of the present invention;
[0025] Figure 5 is a SEM image of the silver powder prepared in Example 5 of the present invention;
[0026] Figure 6 is a SEM image of the silver powder prepared in Example 6 of the present invention;
[0027] Figure 7 is a SEM image of the silver powder prepared in Example 7 of the present invention;
[0028] Figure 8 is a SEM image of the silver powder prepared in Comparative Example 1;
[0029] Fig. 9 This is the SEM image of the silver powder prepared in Comparative Example 1. DETAILED DESCRIPTION
[0030] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0031] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0032] Example 1
[0033] Embodiment 1 provides a method for preparing silver powder, comprising the following steps:
[0034] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3;
[0035] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 200W and the temperature of the silver nitrate solution was room temperature.
[0036] (3) Slowly adding 60-100 nm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining spherical silver powder.
[0037] like Figure 1 As shown, the prepared silver powder is spherical, with a diameter of less than 5 microns and uniform particle size.
[0038] Example 2
[0039] Embodiment 2 provides a method for preparing silver powder, comprising the following steps:
[0040] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3;
[0041] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 200 W and the temperature of the silver nitrate solution was room temperature.
[0042] (3) Slowly adding 5-10 μm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining spherical silver powder.
[0043] like Figure 2 As shown, the prepared silver powder is spherical, with a diameter of less than 5 microns and uniform particle size.
[0044] Example 3
[0045] Embodiment 3 provides a method for preparing silver powder, comprising the following steps:
[0046] Weigh 5 g of AgNO3 powder and add it into deionized water to prepare a saturated solution of AgNO3;
[0047] S1. Use a cell crusher to continuously ultrasonically oscillate the saturated solution of AgNO3 at a power of 200W and a temperature of 10 degrees for the silver nitrate solution.
[0048] S2. Slowly add 60-100 nm copper powder to the saturated solution of AgNO3, and react under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuge the solution at 7000 rpm for 3 minutes, collect the solid matter at the bottom of the centrifuge tube, and obtain spherical silver powder.
[0049] like Figure 3 As shown, the prepared silver powder can obtain flaky silver particles with a diameter of 1 micron and uniform particle size.
[0050] Example 4
[0051] Embodiment 4 provides a method for preparing silver powder, comprising the following steps:
[0052] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3;
[0053] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 200 W and a temperature of 50 degrees Celsius.
[0054] (3) Slowly adding 60-100 nm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining spherical silver powder.
[0055] like Figure 4 As shown, the prepared silver powder is spherical, with a diameter of less than 5 microns and uniform particle size.
[0056] Example 5
[0057] Embodiment 5 provides a method for preparing silver powder, comprising the following steps:
[0058] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3;
[0059] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 100 W and the temperature of the silver nitrate solution was room temperature.
[0060] (3) Slowly adding 60-100 nm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining spherical silver powder.
[0061] like Figure 5 As shown, the prepared silver powder is spherical, with a diameter of less than 10 microns and uniform particle size.
[0062] Example 6
[0063] Embodiment 6 provides a method for preparing silver powder, comprising the following steps:
[0064] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3;
[0065] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 300 W and the temperature of the silver nitrate solution was room temperature.
[0066] (3) Slowly adding 60-100 nm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining spherical silver powder.
[0067] like Figure 6 As shown, the prepared silver powder has a diameter of silver particles less than 5 microns and the particle size is uniform.
[0068] Example 7
[0069] Embodiment 7 provides a method for preparing silver powder, comprising the following steps:
[0070] (1) 5 g of AgNO3 powder was added to deionized water to prepare a saturated solution of AgNO3, and then 50% ethanol was added;
[0071] (2) The saturated solution of AgNO3 was subjected to continuous ultrasonic oscillation using a cell crusher with a power of 200 W and the temperature of the silver nitrate solution was room temperature.
[0072] (3) Slowly adding 60-100 nm copper powder to the saturated solution of AgNO3, and reacting under ultrasonic vibration of a cell crusher; after ultrasonic vibration for 3 minutes, centrifuging the solution at 7000 rpm for 3 minutes, collecting the solid matter at the bottom of the centrifuge tube, and obtaining square silver micron flakes.
[0073] like Figure 7 As shown, the prepared silver powder is in the form of flakes with a diameter of less than 2 microns and a uniform particle size.
[0074] Comparative Example 1
[0075] Comparative Example 1 provides a method for preparing silver powder, and its steps are the same as those of Example 1, except that ultrasound is not used.
[0076] from Figure 8 It can be seen that uniform and fine silver particles cannot be produced, and due to the absence of ultrasound, some copper is not completely reacted, which is quite different from the present invention.
[0077] Comparative Example 2
[0078] Comparative Example 2 provides a method for preparing silver powder, the steps of which are the same as those of Example 1, except that other reducing agents are used instead of copper powder.
[0079] from Fig. 9 It can be seen that silver particles can also be prepared by using ascorbic acid instead of copper powder, but the silver particles are of different sizes and are very uneven, which is quite different from the present invention.
[0080] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A method for preparing silver powder, It is characterized in that The steps include: S1. Ultrasonic vibration is applied to the saturated silver nitrate solution; S2. Under ultrasonic conditions, copper powder and a saturated silver nitrate solution are mixed for reaction, and centrifuged to obtain silver powder; in step S2, the power of the ultrasound is 100-300W; In step S1, the step further includes mixing the ethanol solution and the saturated silver nitrate solution; The volume fraction of the ethanol solution is 30-50%; the temperature of the saturated silver nitrate solution is room temperature.
2. The method for preparing silver powder according to claim 1, It is characterized in that In step S2, the ultrasonic time is 3 to 5 minutes.
3. The method for preparing silver powder according to claim 1, It is characterized in that The mass ratio of the silver nitrate to the copper powder is (2.5-20):
1.
4. The method for preparing silver powder according to claim 1, It is characterized in that The particle size of the copper powder is 10-100000 nm.
5. The method for preparing silver powder according to claim 1, It is characterized in that The centrifugal speed is 1000-7000 rpm.
6. The method for preparing silver powder according to claim 1, It is characterized in that The centrifugation time is 3 to 10 min.