All-solid waste polymerized lightweight soil suitable for large-volume pouring and preparation method and use method thereof
Through the formula of all solid waste polymerization light soil, fly ash, slag powder, steel slag micro powder, caustic soda waste slag and soda ash waste slag are used to reduce the heat of hydration and generate ettringite, which solves the settlement of foam light soil in large volume pouring. Collapse and shrinkage cracking problems, and achieved environmental protection and cost reduction, replacing cement to reduce carbon emissions.
Patent Information
- Application Number
- CN202311503378.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-11-10
AI Technical Summary
Existing foam lightweight soil is prone to settlement, collapse, shrinkage and cracking due to high hydration heat during large volume pouring, and cement production is highly polluted and high carbon emissions, making it difficult to meet the goal of "carbon peak and carbon neutrality".
The all-solid waste polymerization light soil formula is adopted, including fly ash, slag powder, steel slag micro powder, caustic soda waste slag and soda ash waste slag. By reducing the hydration heat of the polymerization reaction, ettringite is generated to compensate for shrinkage, and the foaming agent is used to form. Foam avoids settlement, collapse and cracking, while replacing cement to reduce carbon emissions.
The foam stability and compactness during large-volume pouring have been improved, carbon emissions have been reduced, cement settlement, shrinkage and cracking problems have been avoided, and production costs and energy consumption have been reduced.
Smart Images

Figure CN117623686B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of building materials and solid waste utilization, and in particular to a full-solid waste polymerized lightweight soil suitable for large-volume pouring, and a preparation method and a use method thereof. Background Art
[0002] Guangdong is located in the alluvial plain of the Pearl River Delta. Marine sedimentation has led to widespread soft muddy soil with high organic matter content. If it is not effectively managed, the road-bridge transition section is prone to uneven settlement with the bridgehead road surface under long-term vehicle load, resulting in bridgehead jumping. Foam lightweight soil has unique advantages in dealing with bridgehead jumping, controlling differential settlement of embankment splicing and widening, backfilling in narrow spaces, saving land, etc. It can also simplify the bridge span structure, eliminate the common quality problems of bridgehead jumping, and show good economic efficiency.
[0003] At present, cement is usually used as the cementing material for foam lightweight soil, but the pouring volume of foam lightweight soil usually exceeds 100m 3 , which belongs to large-volume continuous pouring. Due to the high early hydration heat of cement, the large volume of internal heat cannot be effectively removed, resulting in the internal temperature even reaching 70°C. High hydration heat can lead to the following problems: 1) The internal high temperature causes the foam to break easily, thus causing the settlement and collapse of the foam soil (see Figure 1 ); 2) High hydration heat causes foamed lightweight soil to easily cause shrinkage cracking (ref. Figure 1 , Figure 2 ). At the same time, cement production is a high-pollution and high-carbon emission industry. Every ton of ordinary Portland cement produced emits about 0.8 tons of CO2, which does not meet the current national strategic goals of "carbon peak and carbon neutrality". Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a fully solid waste aggregate lightweight soil suitable for large-volume pouring, which can eliminate defects such as sedimentation collapse and cracking, and is environmentally friendly and low-cost.
[0005] The technical problem that the present invention needs to solve is to provide a method for preparing all-solid waste polymer lightweight soil suitable for large-volume casting.
[0006] The technical problem that the present invention needs to solve is to provide a method for using all-solid waste aggregate lightweight soil suitable for large-volume casting.
[0007] The technical problem that the present invention also solves is to provide a fully solid waste aggregated lightweight soil suitable for large-volume pouring and its application in backfilling of roadbed and abutment, soft soil roadbed treatment and road widening.
[0008] In order to solve the above technical problems, the present invention provides a fully solid waste polymerized lightweight soil suitable for large-volume pouring, which comprises the following components in parts by weight: 30-60 parts of fly ash, 10-20 parts of slag powder, 10-20 parts of steel slag powder, 5-20 parts of caustic soda waste residue, 5-15 parts of soda ash waste residue, and 0.02-0.2 parts of foaming agent;
[0009] The main mineral components of the soda ash waste residue are calcium carbonate, calcium sulfate and calcium chloride, and the main mineral components of the caustic soda waste residue are rock salt, mirabilite and caustic soda;
[0010] The total weight of the fly ash, slag powder, steel slag powder, caustic soda waste residue and soda ash waste residue is 100 parts.
[0011] As an improvement of the above technical solution, the fly ash is selected from Class I fly ash or Class II fly ash;
[0012] The slag powder is selected from S75 grade slag powder, S95 grade slag powder or S105 grade slag powder;
[0013] The steel slag powder is selected from primary steel slag powder or secondary steel slag powder.
[0014] As an improvement of the above technical solution, the water content of the caustic soda waste residue is ≥20wt%, and its pH is >12;
[0015] The water content of the soda ash waste residue is ≥10wt%, and the pH value thereof is 8-10.
[0016] As an improvement of the above technical solution, the content of mirabilite in the caustic soda waste residue is ≥70wt%, and the content of rock salt is ≤10wt%.
[0017] As an improvement of the above technical solution, the chemical composition of the soda ash waste residue meets the following relationship:
[0018] LOI 1300 / LOI 1000 =1.22~1.45
[0019] Among them, LOI 1300 LOI is the mass loss rate of absolute dry soda ash waste after calcination to constant weight at 1300℃. 1000 It is the mass loss rate of absolute dry soda ash waste after being burned to constant weight at 1000℃;
[0020] The content of Al2O3 in the fly ash is ≥30wt%, and CaO+MgO+Na2O+K2O+TiO2 is 7-15wt%.
[0021] Correspondingly, the present invention also discloses a method for preparing all-solid waste polymerized lightweight soil suitable for large-volume pouring, which is used to prepare the above-mentioned all-solid waste polymerized lightweight soil suitable for large-volume pouring, and comprises:
[0022] Provide fly ash, slag powder, steel slag powder, caustic soda waste residue, soda ash waste residue and foaming agent respectively, and pack them separately; or
[0023] Provide caustic soda waste residue and soda ash waste residue, mix them to obtain a first mixture; provide fly ash, slag powder and steel slag powder, mix them to obtain a second mixture; provide a foaming agent, and pack the first mixture, the second mixture and the foaming agent separately to obtain the first mixture.
[0024] Correspondingly, the present invention also discloses a method for using the all-solid waste polymerized lightweight soil suitable for large-volume pouring, which is used to use the above-mentioned all-solid waste polymerized lightweight soil suitable for large-volume pouring, and comprises:
[0025] Setting a first slurry pool, adding caustic soda waste residue, soda ash waste residue and a first preset amount of water to prepare a first slurry with a first moisture content;
[0026] Setting a second slurry pool, adding fly ash, slag powder, steel slag powder and a second preset amount of water to prepare a second slurry with a second moisture content;
[0027] Mixing the first slurry and the second slurry evenly to obtain a third slurry;
[0028] The foaming agent is diluted and gas is injected to form a foaming liquid;
[0029] The third slurry is mixed evenly with the foaming liquid and then poured.
[0030] Correspondingly, the present invention also discloses a method for using the all-solid waste polymerized lightweight soil suitable for large-volume pouring, which is used to use the above-mentioned all-solid waste polymerized lightweight soil suitable for large-volume pouring, and comprises:
[0031] A first slurry tank is provided, and a mixture of caustic soda waste residue and soda ash waste residue and a first preset amount of water are added to obtain a first slurry with a first moisture content;
[0032] A second slurry tank is provided, and a mixture of fly ash, slag powder and steel slag powder and a second preset amount of water are added to obtain a second slurry with a second moisture content;
[0033] Mixing the first slurry and the second slurry evenly to obtain a third slurry;
[0034] The foaming agent is diluted and gas is injected to form a foaming liquid;
[0035] The third slurry is mixed evenly with the foaming liquid and then poured.
[0036] As an improvement of the above technical solution, the first moisture content is 60%, and the second moisture content is 60%.
[0037] Correspondingly, the present invention also discloses the application of the above-mentioned all-solid waste polymerized lightweight soil suitable for large-volume pouring in backfilling of roadbed and abutment, soft soil roadbed treatment and road widening.
[0038] The implementation of the present invention has the following beneficial effects:
[0039] 1. The all-solid waste polymerized lightweight soil of the present invention includes 30-60 parts of fly ash, 10-20 parts of slag powder, 10-20 parts of steel slag powder, 5-20 parts of caustic soda waste residue, 5-15 parts of soda ash waste residue, and 0.02-0.2 parts of foaming agent; wherein, both caustic soda waste residue and soda ash waste residue can introduce a certain amount of alkali, thereby effectively reducing the hydration heat of the polymerization reaction, making the internal temperature lower during large-volume pouring, and the internal foam stability is good, which will not cause defoaming, settlement and collapse. In addition, the sulfate ions introduced by the caustic soda waste residue and the calcium ions introduced by the soda ash waste residue can participate in the chemical reaction to form calcium aluminate, and the crystal volume is increased by more than one time, which has the function of compensating for shrinkage, thereby eliminating the shrinkage and cracking problems that are prone to occur in cement foam lightweight soil, and also improving the compactness and strength of the lightweight soil structure.
[0040] 2. The all-solid waste polymer lightweight soil of the present invention includes 30-60 parts of fly ash, 10-20 parts of slag powder, 10-20 parts of steel slag powder, 5-20 parts of caustic soda waste residue, 5-15 parts of soda ash waste residue, and 0.02-0.2 parts of foaming agent; it basically uses all-solid waste materials, can replace cement, can significantly reduce carbon emissions, and is green and environmentally friendly.
[0041] 3. The caustic soda waste residue and soda ash waste residue used in the all-solid waste polymerized lightweight soil of the present invention have a high water content. If they are dried and mixed with other industrial solid wastes, a large amount of energy consumption will be required. At the same time, alkaline materials such as calcium chloride and sodium hydroxide are very easy to absorb water and moisture in the air, resulting in the produced lightweight soil cementing material being easily affected by moisture and deteriorating and unable to be stored for a long time. The preparation and use method of the polymerized lightweight soil mentioned in the present invention eliminates the drying step, which on the one hand reduces the cost of the polymerized lightweight soil, and on the other hand can also solve the problem that the polymerized lightweight soil cementing material containing alkaline materials is easily affected by moisture and cannot be stored for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a real shot of the defects of large-volume pouring of lightweight soil in the prior art;
[0043] Figure 2 This is a real shot of another defect in the prior art of pouring lightweight soil in large volumes;
[0044] Figure 3This is a real shot of the all-solid waste aggregate lightweight soil in one embodiment of the present invention after 28 days of pouring. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below in conjunction with specific implementation methods.
[0046] The present invention provides a fully solid waste polymerized lightweight soil, which comprises the following components in parts by weight:
[0047] 30-60 parts of fly ash, 10-20 parts of slag powder, 10-20 parts of steel slag powder, 5-20 parts of caustic soda waste residue, 5-15 parts of soda ash waste residue, and 0.02-0.2 parts of foaming agent.
[0048] Among them, fly ash is the solid waste collected in the flue gas after coal combustion. It contains Si-Al-Na(K)-Ca(Mg) glass, which is highly active and can provide silicon source and calcium source to form hydrated calcium silicate through hydration reaction. Moreover, hydrated calcium silicate will further react with caustic soda waste residue and soda ash waste residue to form calcium aluminate, which can compensate for hydration shrinkage and improve the compactness and strength of lightweight soil structure. Specifically, in the present invention, fly ash can be Class I fly ash or Class II fly ash, and its usage is 30 to 60 parts, exemplarily 35 parts, 40 parts, 45 parts, 50 parts or 55 parts, but not limited thereto.
[0049] Preferably, in one embodiment of the present invention, the content of Al2O3 in fly ash is ≥30wt%, and CaO+MgO+Na2O+K2O+TiO2=7-15wt% (i.e., the sum of the content of CaO, the content of MgO, the content of Na2O, the content of K2O and the content of TiO2 in fly ash). In the fly ash based on the above chemical composition, a large amount of Al exists in the form of glass, and the crystalline phase Al (such as corundum, mullite, etc.) is relatively small, which is easier to react with caustic soda waste residue and soda ash waste residue to form calcium aluminate, reduce hydration heat, compensate for hydration shrinkage and improve strength. Specifically, the content of Al2O3 in fly ash is 35-50wt%, exemplified by 37wt%, 38wt%, 40wt%, 43wt%, 45wt% or 48wt%, but not limited thereto.
[0050] Among them, slag powder is a powder material obtained by grinding granulated blast furnace slag to a specified fineness. It has high potential activity and can undergo hydration reaction under alkaline excitation conditions to improve the strength of lightweight soil. Specifically, in the present invention, the grade of slag powder is not lower than S75 grade. Specifically, S75 grade slag powder, S95 grade slag powder or S105 grade slag powder can be selected, but not limited to this. The amount of slag powder is 10 to 20 parts, exemplarily 12 parts, 14 parts, 16 parts or 18 parts, but not limited to this.
[0051] Among them, the steel slag powder is a powder obtained by grinding the waste slag produced in the process of converter or electric furnace ironmaking, which contains silicate and ferrite and has certain activity. Specifically, in the present invention, the steel slag powder is selected from the first-grade steel slag powder or the second-grade steel slag powder, but it is not limited thereto. The amount of steel slag powder is 10 to 20 parts, exemplarily 12 parts, 14 parts, 16 parts or 18 parts, but it is not limited thereto.
[0052] Among them, caustic soda waste residue is the waste residue generated in the production process of caustic soda (NaOH), specifically the waste residue generated by membrane denitrification in the process of preparing caustic soda by ion membrane method, and its main mineral phase components are rock salt, mirabilite and caustic soda, and it contains a large amount of free alkali (pH ≥ 11), which can be used as an alkali activator to dissolve and activate active components such as vitreous body, provide strength, reduce hydration heat, and avoid defects such as cracks and sedimentation. Specifically, the amount of caustic soda waste residue is 5 to 20 parts, and exemplary ones are 8 parts, 11 parts, 13 parts, 17 parts or 19 parts, but not limited thereto.
[0053] Preferably, in one embodiment of the present invention, the water content of the caustic soda waste residue is ≥10wt%, and the pH is >12. More preferably, the water content of the caustic soda is ≥20wt%, and the content of free caustic soda in such caustic soda waste residue is higher, which can better activate the active components. More specifically, the water content of the caustic soda waste residue is 20-40wt%, exemplarily 24wt%, 28wt%, 30wt%, 34wt% or 37wt%, but not limited thereto. The pH of the caustic soda waste residue is 12-14, exemplarily 12.5, 13 or 13.5, but not limited thereto.
[0054] Preferably, in one embodiment of the present invention, the content of mirabilite in the caustic soda waste residue is ≥70wt%, and the content of rock salt is ≤10wt%. Based on the above-mentioned caustic soda waste residue, the content of calcium sulfate in the polymer lightweight soil can be effectively increased, and the strength can be improved; at the same time, the adverse effects of free chloride ions can be reduced. Specifically, the content of mirabilite in the caustic soda waste residue is 75-85wt%, and exemplarily 76wt%, 78wt%, 80wt%, 82wt% or 84wt%, but not limited thereto. The content of rock salt in the caustic soda waste residue is 5-10wt%, and exemplarily 5.5wt%, 7wt%, 8wt% or 9.5wt%, but not limited thereto. It should be noted that the content of mirabilite and the content of rock salt here refer to the content of mirabilite and the content of rock salt in the absolutely dry caustic soda waste residue, and the absolutely dry caustic soda waste residue is obtained by drying the caustic soda waste residue to constant weight at 50-120°C.
[0055] Among them, soda ash waste residue is the waste residue produced in the process of producing soda ash, and its main mineral components are calcium carbonate, calcium sulfate and calcium chloride. Soda ash waste residue is the main source of Ca to form more calcium sulfate and improve the strength of lightweight soil. Specifically, the amount of soda ash waste residue is 5 to 15 parts, exemplarily 6 parts, 8 parts, 10 parts or 12 parts, but not limited thereto.
[0056] The water content of the soda ash waste residue is ≥10wt%, preferably 10-40wt%. Based on the preparation method and use method of the present invention, the soda ash waste residue can be effectively utilized without dehydration or drying.
[0057] Preferably, in one embodiment of the present invention, the chemical composition of the soda ash waste residue meets the following relationship:
[0058] LOI 1300 / LOI 1000 =1.22~1.45
[0059] Among them, LOI 1300 LOI is the mass loss rate of absolute dry soda ash waste after calcination to constant weight at 1300℃. 1000 It is the mass loss rate of absolute dry soda ash waste slag after burning to constant weight at 1000℃, wherein the absolute dry soda ash waste slag is obtained by drying the soda ash waste slag to constant weight at 50-120℃. In the caustic soda waste slag based on this chemical composition, the content of mineral phase component calcium sulfate is relatively high, which can effectively increase the content of ettringite after solidification, reduce hydration heat, compensate for hydration shrinkage and improve strength.
[0060] The foaming agent may be one or more of a rosin foaming agent, a protein foaming agent, and a composite foaming agent, but is not limited thereto. When used, the foaming agent needs to be dispersed and diluted with water, and injected with gas to form foam, and then used in the form of a foaming liquid. The apparent density of the foaming liquid is 40 to 60 g / L.
[0061] Specifically, the amount of the foaming agent is 0.02 to 0.2 parts, exemplified by 0.02 parts, 0.05 parts, 0.08 parts, 0.12 parts, 0.15 parts or 0.18 parts, but not limited thereto.
[0062] Correspondingly, the present invention also discloses a method for preparing all-solid waste polymerized lightweight soil suitable for large-volume pouring, which comprises: providing fly ash, slag powder, steel slag powder, caustic soda waste slag, soda ash waste slag and foaming agent respectively, and packaging them respectively. Alternatively, caustic soda waste slag and soda ash waste slag can be mixed to obtain a first mixture; fly ash, slag powder and steel slag powder can be mixed to obtain a second mixture; and then the first mixture, the second mixture and the foaming agent can be packaged respectively to obtain.
[0063] Correspondingly, the present invention also discloses a method for using all-solid waste polymerized lightweight soil suitable for large-volume pouring, which comprises the following steps:
[0064] (1) A first slurry tank is set up, and caustic soda waste residue, soda ash waste residue and a first preset amount of water are added to prepare a first slurry with a first moisture content; wherein the first moisture content is 45-65%, preferably 60%.
[0065] (2) Setting up a second slurry pool, adding fly ash, slag powder, steel slag powder and a second preset amount of water to prepare a second slurry with a second moisture content; wherein the second moisture content is 45-65%, preferably 60%.
[0066] (3) uniformly mixing the first slurry and the second slurry to obtain a third slurry;
[0067] The first slurry and the second slurry may be mixed in the second slurry tank, or a third slurry tank may be provided to mix the two slurries in the third slurry tank.
[0068] (4) diluting the foaming agent and injecting gas to foam it to form a foaming liquid;
[0069] (5) Mix the third slurry and the foaming liquid evenly and then pour.
[0070] Correspondingly, the present invention also discloses another method for using all-solid waste polymerized lightweight soil suitable for large-volume pouring, which comprises the following steps:
[0071] (1) A first slurry tank is provided, and a mixture of caustic soda waste residue and soda ash waste residue and a first preset amount of water are added to obtain a first slurry with a first moisture content; wherein the first moisture content is 45-65%, preferably 60%.
[0072] (2) Setting up a second slurry pool, adding a mixture of fly ash, slag powder and steel slag powder and a second preset amount of water to obtain a second slurry with a second moisture content; wherein the second moisture content is 45-65%, preferably 60%.
[0073] (3) uniformly mixing the first slurry and the second slurry to obtain a third slurry;
[0074] The first slurry and the second slurry may be mixed in the second slurry tank, or a third slurry tank may be provided to mix the two slurries in the third slurry tank.
[0075] (4) diluting the foaming agent and injecting gas to foam it to form a foaming liquid;
[0076] (5) Mix the third slurry and the foaming liquid evenly and then pour.
[0077] The present invention is described below with specific embodiments:
[0078] The present invention will be further described below with specific embodiments:
[0079] Example 1
[0080] This embodiment provides a fully solid waste polymerized lightweight soil suitable for large-volume pouring, and its formula is as follows:
[0081] 60 parts of Class I fly ash, 10 parts of S75 grade slag powder, 10 parts of Class I steel slag powder, 10 parts of caustic soda waste residue, 10 parts of soda ash waste residue, and 0.05 parts of foaming agent.
[0082] Among them, the chemical composition of grade I fly ash is: SiO2 50.3%, Al2O3 28.63%, Fe2O3 4.58%, TiO21.61%, CaO 1.78%, MgO 0.47%, Na2O 0.46%, K2O 1.4%, LOI (1000℃) 10.77%.
[0083] The water content of the caustic soda waste residue is 35.4wt%, the pH value is 12.5, the content of mirabilite in the absolutely dry caustic soda waste residue is 65.5wt%, the content of rock salt is 20.3wt%, and the content of caustic soda is 14.2wt%.
[0084] The water content of soda ash waste is 30.5wt%, and its LOI 1300 24.5wt%, LOI 1000 It is 16.7wt%.
[0085] The method of using the method is as follows: caustic soda waste residue, soda ash waste residue and water are mixed evenly to obtain a first slurry with a water content of 60wt%; fly ash, slag powder, steel slag powder and water are mixed evenly to obtain a second slurry with a water content of 60wt%; the first slurry and the second slurry are mixed to obtain a third slurry; a foaming agent is dispersed and diluted with water, and gas is injected to foam to form foam, and then used in the form of a foaming liquid. The apparent density of the foaming liquid is 50g / L. The foaming liquid and the third slurry are mixed evenly and then poured.
[0086] Example 2
[0087] This embodiment provides a fully solid waste polymerized lightweight soil suitable for large-volume pouring, and its formula is as follows:
[0088] 55 parts of Class I fly ash, 12 parts of S95 grade slag powder, 13 parts of Class I steel slag powder, 12 parts of caustic soda waste residue, 8 parts of soda ash waste residue, and 0.05 parts of foaming agent.
[0089] Among them, the chemical composition of grade I fly ash is: SiO2 50.3%, Al2O3 28.63%, Fe2O3 4.58%, TiO21.61%, CaO 1.78%, MgO 0.47%, Na2O 0.46%, K2O 1.4%, LOI (1000℃) 10.77%.
[0090] The water content of the caustic soda waste residue is 39.6wt%, the pH value is 13, the content of mirabilite in the absolutely dry caustic soda waste residue is 78.3wt%, the content of rock salt is 7.1wt%, and the content of caustic soda is 14.6wt%.
[0091] The water content of soda ash waste is 30.5wt%, and its LOI 1300 24.5wt%, LOI 1000 It is 16.7wt%.
[0092] Its usage is the same as that of Example 1.
[0093] Example 3
[0094] This embodiment provides a fully solid waste polymerized lightweight soil suitable for large-volume pouring, which differs from Embodiment 2 in that:
[0095] The chemical composition of grade I fly ash is: SiO2 49.04%, Al2O3 38.26%, Fe2O3 2.18%, TiO2 2.54%, CaO 3.21%, MgO 0.26%, Na2O 1.47%, K2O 0.72%, LOI (1000℃) 2.32%.
[0096] The rest are the same as in Example 2.
[0097] Example 4
[0098] This embodiment provides a fully solid waste polymerized lightweight soil suitable for large-volume pouring, which differs from Embodiment 3 in that:
[0099] The water content of soda ash waste is 28.5wt%, and its LOI 1300 LOI is 21.9% 1000 It is 15.9wt%.
[0100] Comparative Example 1
[0101] This comparative example provides a polymerized lightweight soil, which differs from Example 1 in that the formula does not contain caustic soda waste residue, and the rest is the same as Example 1.
[0102] Comparative Example 2
[0103] This comparative example provides a polymerized lightweight soil, which differs from Example 1 in that the formula does not contain soda ash waste residue, and the rest is the same as Example 1.
[0104] Comparative Example 3
[0105] This comparative example provides a polymerized lightweight soil, which differs from Example 1 in that the formula does not contain caustic soda waste residue and soda ash waste residue, and the rest is the same as Example 1.
[0106] The polymerized lightweight soils in Examples 1 to 4 and Comparative Examples 1 to 3 were poured and their various properties were tested. The specific testing methods are as follows:
[0107] (1) The unconfined compressive strength test is based on the Technical Specification for Cast-in-place Foam Lightweight Soil (CECS 249-2008);
[0108] (2) Center temperature: A scaled cube model of 7 m × 8 m × 0.5 m was cast, and a temperature sensor was attached at the position of 0.35 m × 0.4 m × 0.25 m. The standard curing environment was maintained and the center temperature of the lightweight soil was continuously monitored. The average temperature on the third day was taken and recorded as the center temperature.
[0109] (3) The freeze-thaw cycle test and shrinkage test refer to the standard "Test Code for Cement and Cement Concrete for Highway Engineering" (JTG 3420-2020).
[0110] The specific results are as follows:
[0111]
[0112] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A fully solid waste aggregate lightweight soil suitable for large volume pouring, It is characterized in that The invention is composed of the following components in parts by weight: 30-60 parts of fly ash, 10-20 parts of slag powder, 10-20 parts of steel slag powder, 5-20 parts of caustic soda waste residue, 5-15 parts of soda ash waste residue, and 0.02-0.2 parts of foaming agent; The total weight of the fly ash, slag powder, steel slag powder, caustic soda waste residue and soda ash waste residue is 100 parts; Wherein, the main mineral components of the soda ash waste slag are calcium carbonate, calcium sulfate and calcium chloride; The main mineral components of the caustic soda waste slag are rock salt, mirabilite and caustic soda, and the content of mirabilite is ≥70wt%, and the content of rock salt is ≤10wt%; The chemical composition of the soda ash waste residue meets the following relationship: Among them, LOI 1300 LOI is the mass loss rate of absolute dry soda ash waste after calcination to constant weight at 1300℃. 1000 It is the mass loss rate of absolute dry soda ash waste after burning to constant weight at 1000℃; The Al in fly ash 2 O 3 Content ≥30wt%, CaO+MgO+Na 2 O+K 2 O+TiO 2 =7~15wt%.
2. The all-solid waste aggregate lightweight soil suitable for large-volume pouring as claimed in claim 1, It is characterized in that The fly ash is selected from Class I fly ash or Class II fly ash; The slag powder is selected from S75 grade slag powder, S95 grade slag powder or S105 grade slag powder; The steel slag powder is selected from primary steel slag powder or secondary steel slag powder.
3. The all-solid waste aggregate lightweight soil suitable for large-volume pouring as claimed in claim 1, It is characterized in that The caustic soda waste residue has a moisture content of ≥20wt% and a pH value of >12; The water content of the soda ash waste residue is ≥10wt%, and its pH is 8-10.
4. A method for preparing all-solid waste polymerized lightweight soil suitable for large-volume pouring, for preparing the all-solid waste polymerized lightweight soil suitable for large-volume pouring as claimed in any one of claims 1 to 3, It is characterized in that include: Provide fly ash, slag powder, steel slag powder, caustic soda waste residue, soda ash waste residue and foaming agent respectively, and pack them respectively to obtain; or Provide caustic soda waste residue and soda ash waste residue, mix them to obtain a first mixture; provide fly ash, slag powder and steel slag powder, mix them to obtain a second mixture; provide a foaming agent, and pack the first mixture, the second mixture and the foaming agent separately to obtain the first mixture.
5. A method for using all-solid waste polymerized lightweight soil suitable for large-volume pouring, for using the all-solid waste polymerized lightweight soil suitable for large-volume pouring as claimed in any one of claims 1 to 3, It is characterized in that include: Setting a first slurry pool, adding caustic soda waste residue, soda ash waste residue and a first preset amount of water to prepare a first slurry with a first moisture content; Setting a second slurry pool, adding fly ash, slag powder, steel slag powder and a second preset amount of water to prepare a second slurry with a second moisture content; Mixing the first slurry and the second slurry evenly to obtain a third slurry; The foaming agent is diluted and gas is injected to form a foaming liquid; The third slurry is mixed evenly with the foaming liquid and then poured.
6. A method for using all-solid waste polymerized lightweight soil suitable for large-volume pouring, for using the all-solid waste polymerized lightweight soil suitable for large-volume pouring as claimed in any one of claims 1 to 3, It is characterized in that include: A first slurry tank is provided, and a mixture of caustic soda waste residue and soda ash waste residue and a first preset amount of water are added to obtain a first slurry with a first moisture content; A second slurry tank is provided, and a mixture of fly ash, slag powder and steel slag powder and a second preset amount of water are added to obtain a second slurry with a second moisture content; Mixing the first slurry and the second slurry evenly to obtain a third slurry; The foaming agent is diluted and gas is injected to form a foaming liquid; The third slurry is mixed evenly with the foaming liquid and then poured.
7. The method for using the all-solid waste aggregate lightweight soil suitable for large-volume pouring as claimed in claim 5 or 6, It is characterized in that The first moisture content is 60%, and the second moisture content is 60%.
8. Application of the all-solid waste aggregate lightweight soil suitable for large-volume casting as described in any one of claims 1 to 3 in backfilling of roadbed and abutment, soft soil roadbed treatment and road widening.
Citation Information
Patent Citations
Foam light soil material applied to large-scale filling projects, and preparation method thereof
CN110304877A
Alkali residue light soil as well as preparation method and application thereof
CN116119999A