A basalt insulating composite material and its application in operating rod
By modifying basalt fiber and pre-reaction to form a network structure, combined with epoxy resin for curing, it solves the problem of insufficient strength and electrical breakdown performance of existing basalt fiber-epoxy resin composite materials, and significantly improves the performance and performance of insulating composite materials. service life.
Patent Information
- Application Number
- CN202311707725.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-13
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to a basalt insulating composite material and application thereof in an operating rod. Background Art
[0002] The insulated operating rod is a commonly used working equipment in the maintenance of high-voltage transmission line circuits. It is mainly made of glass fiber and epoxy resin through pultrusion, winding or tube rolling process. Its materials mainly include glass fiber and epoxy resin materials. However, the glass fiber epoxy resin material has low strength, is prone to aging after long-term use, and has a short service life, which seriously limits its application.
[0003] Basalt fiber BF is the abbreviation of basalt fiber. Compared with carbon fiber, aramid and ultra-high molecular weight polyethylene fiber, basalt fiber has the characteristics of high strength and high modulus. It also has excellent properties such as good high temperature resistance, oxidation resistance and radiation resistance. The existing insulating operating rod materials use basalt fiber to replace the original glass fiber to improve the strength and electrical breakdown performance of the material. However, due to the poor compatibility between basalt fiber and epoxy resin and limited interface bonding strength, the improvement effect of material strength and electrical breakdown performance is limited. Summary of the invention
[0004] In order to overcome the defects of the existing basalt fiber epoxy resin composite material in terms of limited strength and electrical breakdown performance, a basalt insulating composite material and its application in an operating rod are provided.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A basalt insulating composite material, the preparation method of which comprises the following steps:
[0007] 1) mixing basalt fiber, a silane coupling agent and a first solvent, stirring, filtering after the stirring, drying and crushing to obtain amino-modified basalt fiber;
[0008] 2) mixing the amino-modified basalt fiber, trimesic acid and the second solvent, and stirring to obtain a first mixed solution;
[0009] 3) mixing 2-amino-4,4'-biphenyldicarboxylic acid, 1-dodecyloxy-2,4-phenylenediamine and a second solvent, then adding sodium hypophosphite, heating to react under a nitrogen atmosphere, and after the heating reaction is completed, adding the first mixed solution to mix, to obtain a second mixed solution;
[0010] 4) filtering the second mixed solution, spinning after degassing to obtain primary fibers, and then heat treating, drawing, and shearing the primary fibers to obtain modified fibers;
[0011] 5) Mixing the epoxy resin and the modified fiber obtained in step 4), then adding a curing agent and heating and curing to obtain the basalt insulation composite material.
[0012] Preferably, in step 1), the mass ratio of basalt fiber, silane coupling agent and first solvent is 100:(12-25):(200-400);
[0013] The first solvent is selected from water and ethanol, and the mass ratio of water to ethanol is 1:(1-3).
[0014] Preferably, in step 1), the stirring temperature is 70-85° C. and the stirring time is 1-5 h.
[0015] Preferably, in step 2), the mass ratio of the amino-modified basalt fiber, trimesic acid and the second solvent is 100:(15-30):(100-200);
[0016] Step 2) The stirring temperature is 80-90°C and the stirring time is 1-4h.
[0017] Preferably, the second solvent is selected from one of N,N-dimethylacetamide and N,N-dimethylformamide.
[0018] Preferably, in step 3), the molar ratio of 2-amino-4,4'-biphenyldicarboxylic acid to 1-dodecyloxy-2,4-phenylenediamine is 1:(1-1.3);
[0019] In step 3), the amount of the second solvent added is 1.5-3 times the mass of 2-amino-4,4'-biphenyldicarboxylic acid;
[0020] The amount of sodium hypophosphite added is 2%-8% of the mass of 2-amino-4,4'-biphenyldicarboxylic acid.
[0021] Preferably, in step 3), the heating reaction temperature is 90-98° C., and the heating reaction time is 1-4 h.
[0022] Preferably, in step 4), nitrogen gas at 240-260° C. is introduced during the spinning process to volatilize the solvent;
[0023] In step 4), the heat treatment temperature is 320-360° C. and the heat treatment time is 1-3 h;
[0024] In step 4), the stretching ratio is 1.0-2.0 times, and the stretching temperature is 420-460°C.
[0025] Preferably, in step 5), the mass ratio of epoxy resin to modified fiber is 100:(30-45);
[0026] In step 5), the amount of curing agent added is 30%-50% of the mass of the epoxy resin;
[0027] The epoxy resin is selected from epoxy resin E51, and the curing agent is selected from epoxy resin curing agent T31;
[0028] The heating and curing step in step 5) includes first curing at 120-150° C. for 3-8 hours, then cooling to 80-90° C. and continuing curing for 10-20 hours.
[0029] The present invention also provides application of the above-mentioned basalt insulating composite material in an operating rod.
[0030] Beneficial effects of the present invention:
[0031] The basalt insulation composite material provided by the present invention has a preparation method, wherein firstly, basalt fiber is modified by a silane coupling agent to obtain amino-modified basalt fiber, and the amino-modified basalt fiber and trimesic acid are pre-reacted to obtain a first mixed solution; then 2-amino-4,4'-biphenyldicarboxylic acid and 1-dodecyloxy-2,4-phenylenediamine are pre-reacted, and the reaction solution is mixed with the first mixed solution to obtain a second mixed solution; the second mixed solution is spun and heat-treated, and a cross-linking reaction is further performed during the heat treatment process to obtain modified fiber; and finally, epoxy resin and the modified fiber are cured to obtain the basalt insulation composite material. In the preparation method of the present invention, 2-amino-4,4'-biphenyldicarboxylic acid and 1-dodecyloxy-2,4-phenylenediamine are used for prepolymerization, and then the prepolymerization product is cross-linked with amino-modified basalt fiber through trimesic acid to form a unique mesh structure, which tightly wraps the basalt fiber. At the same time, dodecyloxy groups are introduced to increase the compatibility with epoxy resin and improve the strength and electrical breakdown performance of the composite material. The composite material obtained by the present invention has excellent strength and electrical breakdown performance, and the volume resistance of the composite material is 10 12 Ω·m and above, and also has excellent insulation performance. DETAILED DESCRIPTION
[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0033] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0034] Example 1
[0035] This embodiment provides a basalt insulation composite material, and the preparation method of the basalt insulation composite material includes the following steps:
[0036] 1) 100 g of basalt fiber, 15 g of silane coupling agent KH550, 150 g of water and 200 g of ethanol were mixed, stirred at 85° C. for 3 h, and after the stirring and mixing, filtered, dried and crushed to obtain amino-modified basalt fiber;
[0037] 2) 100 g of amino-modified basalt fiber, 20 g of trimesic acid and 150 g of N,N-dimethylacetamide were mixed, and stirred at 80° C. for 1.5 h to obtain a first mixed solution;
[0038] 3) 25 g of 2-amino-4,4'-biphenyldicarboxylic acid, 30 g of 1-dodecyloxy-2,4-phenylenediamine, and 50 g of N,N-dimethylacetamide were mixed, and then 0.5 g of sodium hypophosphite was added, and heated to react under a nitrogen atmosphere at a temperature of 95° C. for 1.5 h. After the heating reaction was completed, the first mixed solution was added and mixed to obtain a second mixed solution;
[0039] 4) filtering the second mixed solution, degassing and sending it into a dry spinning tunnel for spinning, introducing nitrogen at 260° C. to volatilize the solvent to obtain spun fibers, and then heat-treating the spun fibers at 340° C. for 1.5 h, and then drawing them at 450° C. by 1.5 times, and shearing them to obtain modified fibers;
[0040] 5) 100 g of epoxy resin E51 and 35 g of the modified fiber obtained in step 4) were mixed, and then 40 g of epoxy resin curing agent T31 was added, and the mixture was cured at 130° C. for 4 h, and then cooled to 80° C. and further cured for 10 h to obtain the basalt insulation composite material.
[0041] Example 2
[0042] This embodiment provides a basalt insulation composite material, and the preparation method of the basalt insulation composite material includes the following steps:
[0043] 1) 100 g of basalt fiber, 18 g of silane coupling agent KH550, 150 g of water and 200 g of ethanol were mixed, stirred at 82° C. for 4 h, and after the stirring and mixing, filtered, dried and crushed to obtain amino-modified basalt fiber;
[0044] 2) 100 g of amino-modified basalt fiber, 25 g of trimesic acid and 150 g of N,N-dimethylacetamide were mixed, and stirred at 80° C. for 3 h to obtain a first mixed solution;
[0045] 3) 25 g of 2-amino-4,4'-biphenyldicarboxylic acid, 35 g of 1-dodecyloxy-2,4-phenylenediamine, and 50 g of N,N-dimethylacetamide were mixed, and then 1.5 g of sodium hypophosphite was added, and heated to react under a nitrogen atmosphere at a temperature of 95° C. for 2.5 h. After the heating reaction was completed, the first mixed solution was added and mixed to obtain a second mixed solution;
[0046] 4) filtering the second mixed solution, degassing and sending it into a dry spinning tunnel for spinning, introducing nitrogen at 260° C. to volatilize the solvent to obtain spun fibers, and then heat-treating the spun fibers at 340° C. for 2 h, and then stretching them by 1.5 times at 450° C. and shearing them to obtain modified fibers;
[0047] 5) 100 g of epoxy resin E51 and 40 g of the modified fiber obtained in step 4) were mixed, and then 40 g of epoxy resin curing agent T31 was added, and the mixture was cured at 130° C. for 4 h, and then cooled to 80° C. and further cured for 10 h to obtain the basalt insulation composite material.
[0048] Example 3
[0049] This embodiment provides a basalt insulation composite material, and the preparation method of the basalt insulation composite material includes the following steps:
[0050] 1) 100 g of basalt fiber, 16 g of silane coupling agent KH550, 150 g of water and 200 g of ethanol were mixed, stirred at 82° C. for 4 h, and after the stirring and mixing, filtered, dried and crushed to obtain amino-modified basalt fiber;
[0051] 2) 100 g of amino-modified basalt fiber, 23 g of trimesic acid and 150 g of N,N-dimethylacetamide were mixed, and stirred at 80° C. for 3 h to obtain a first mixed solution;
[0052] 3) 25 g of 2-amino-4,4'-biphenyldicarboxylic acid, 32 g of 1-dodecyloxy-2,4-phenylenediamine, and 50 g of N,N-dimethylacetamide were mixed, and then 1.1 g of sodium hypophosphite was added, and heated to react under a nitrogen atmosphere at a temperature of 95° C. for 2.5 h. After the heating reaction was completed, the first mixed solution was added and mixed to obtain a second mixed solution;
[0053] 4) filtering the second mixed solution, degassing and sending it into a dry spinning tunnel for spinning, introducing nitrogen at 260° C. to volatilize the solvent to obtain spun fibers, and then heat-treating the spun fibers at 340° C. for 2 h, and then stretching them by 1.5 times at 460° C. and shearing them to obtain modified fibers;
[0054] 5) 100 g of epoxy resin E51 and 37 g of the modified fiber obtained in step 4) were mixed, and then 40 g of epoxy resin curing agent T31 was added, and the mixture was cured at 130° C. for 4.5 h, and then the mixture was cooled to 80° C. and further cured for 10 h to obtain the basalt insulation composite material.
[0055] Example 4
[0056] This embodiment provides a basalt insulation composite material, and the preparation method of the basalt insulation composite material includes the following steps:
[0057] 1) 100 g of basalt fiber, 20 g of silane coupling agent KH550, 150 g of water and 200 g of ethanol were mixed, stirred at 82° C. for 4 h, and after the stirring and mixing, filtered, dried and crushed to obtain amino-modified basalt fiber;
[0058] 2) 100 g of amino-modified basalt fiber, 28 g of trimesic acid and 150 g of N,N-dimethylacetamide were mixed, and stirred at 80° C. for 3.5 h to obtain a first mixed solution;
[0059] 3) 25 g of 2-amino-4,4'-biphenyldicarboxylic acid, 40 g of 1-dodecyloxy-2,4-phenylenediamine, and 50 g of N,N-dimethylacetamide were mixed, and then 1.5 g of sodium hypophosphite was added, and heated to react under a nitrogen atmosphere at a temperature of 95° C. for 3 h. After the heating reaction was completed, the first mixed solution was added and mixed to obtain a second mixed solution;
[0060] 4) filtering the second mixed solution, degassing and sending it into a dry spinning tunnel for spinning, introducing nitrogen at 260° C. to volatilize the solvent to obtain spun fibers, and then heat-treating the spun fibers at 340° C. for 2.5 h, and then stretching them by 1.5 times at 450° C. and shearing them to obtain modified fibers;
[0061] 5) 100 g of epoxy resin E51 and 44 g of the modified fiber obtained in step 4) were mixed, and then 40 g of epoxy resin curing agent T31 was added, and the mixture was cured at 130° C. for 4 h, and then cooled to 80° C. and further cured for 10 h to obtain the basalt insulation composite material.
[0062] Comparative Example 1
[0063] This comparative example provides a basalt insulation composite material, and the preparation method of the basalt insulation composite material comprises the following steps:
[0064] 100 g of epoxy resin E51 and 35 g of basalt fiber were mixed, and then 40 g of epoxy resin curing agent T31 was added, and the mixture was cured at 130° C. for 4 hours, and then the mixture was cooled to 80° C. and cured for 10 hours to obtain the basalt insulation composite material.
[0065] Comparative Example 2
[0066] This comparative example provides a basalt insulating composite material, which is different from Example 1 in that in step 3), 25g of 2-amino-4,4'-biphenyldicarboxylic acid, 11.1g of 1,3-phenylenediamine and 50g of N,N-dimethylacetamide are mixed, and then 0.5g of sodium hypophosphite is added, and a heating reaction is carried out under a nitrogen atmosphere. The heating reaction temperature is 95°C and the heating reaction time is 1.5h. After the heating reaction is completed, the first mixed solution is added and mixed to obtain a second mixed solution.
[0067] Comparative Example 3
[0068] This comparative example provides a basalt insulating composite material, which is different from Example 1 in that in step 3), 23.5 g of 4,4'-biphenyldicarboxylic acid, 30 g of 1-dodecyloxy-2,4-phenylenediamine and 50 g of N,N-dimethylacetamide are mixed, and then 0.5 g of sodium hypophosphite is added, and a heating reaction is carried out under a nitrogen atmosphere. The heating reaction temperature is 95° C. and the heating reaction time is 1.5 h. After the heating reaction is completed, the first mixed solution is added and mixed to obtain a second mixed solution.
[0069] Test Case
[0070] The basalt insulating composite materials prepared in the above examples and comparative examples were subjected to performance tests, wherein the flexural modulus and flexural strength were tested in accordance with standard GB / T 1449-2005, and the electrical breakdown strength was tested in accordance with standard GB1408-1989. The test results are shown in Table 1.
[0071] Table 1
[0072] Flexural modulus / GPa Bending strength / MPa Electrical breakdown strength kv / mm Example 1 96.4 602.7 35.43 Example 2 98.9 607.1 35.50 Example 3 97.2 605.4 35.45 Example 4 99.7 610.6 35.52 Comparative Example 1 87.2 570.6 34.88 Comparative Example 2 93.6 594.5 35.39 Comparative Example 3 89.7 579.8 35.16
[0073] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A basalt insulating composite material, characterized in that: The preparation method thereof comprises the following steps: 1) mixing basalt fiber, a silane coupling agent and a first solvent, stirring, filtering after the stirring, drying and crushing to obtain amino-modified basalt fiber; 2) mixing the amino-modified basalt fiber, trimesic acid and the second solvent, and stirring to obtain a first mixed solution; 3) mixing 2-amino-4,4'-biphenyldicarboxylic acid, 1-dodecyloxy-2,4-phenylenediamine and a second solvent, then adding sodium hypophosphite, heating to react under a nitrogen atmosphere, and after the heating reaction is completed, adding the first mixed solution to mix, to obtain a second mixed solution; 4) filtering the second mixed solution, spinning after degassing to obtain primary fibers, and then heat treating, drawing, and shearing the primary fibers to obtain modified fibers; 5) mixing the epoxy resin and the modified fiber obtained in step 4), then adding a curing agent and heating and curing to obtain the basalt insulation composite material; The silane coupling agent is silane coupling agent KH550.
2. The basalt insulating composite material according to claim 1, characterized in that: In step 1), the mass ratio of basalt fiber, silane coupling agent and first solvent is 100:(12-25):(200-400); The first solvent is selected from water and ethanol, and the mass ratio of water to ethanol is 1:(1-3).
3. The basalt insulating composite material according to claim 1 or 2, characterized in that: In step 1), the stirring temperature is 70-85° C. and the stirring time is 1-5 h.
4. The basalt insulating composite material according to claim 1, characterized in that: In step 2), the mass ratio of amino-modified basalt fiber, trimesic acid and the second solvent is 100:(15-30):(100-200); Step 2) The stirring temperature is 80-90°C and the stirring time is 1-4h.
5. The basalt insulating composite material according to claim 1, characterized in that: The second solvent is selected from one of N,N-dimethylacetamide and N,N-dimethylformamide.
6. The basalt insulating composite material according to claim 1, characterized in that: In step 3), the molar ratio of 2-amino-4,4'-biphenyldicarboxylic acid to 1-dodecyloxy-2,4-phenylenediamine is 1:(1-1.3); In step 3), the amount of the second solvent added is 1.5-3 times the mass of 2-amino-4,4'-biphenyldicarboxylic acid; The amount of sodium hypophosphite added is 2%-8% of the mass of 2-amino-4,4'-biphenyldicarboxylic acid.
7. The basalt insulating composite material according to claim 1, characterized in that: In step 3), the heating reaction temperature is 90-98° C. and the heating reaction time is 1-4 h.
8. The basalt insulating composite material according to claim 1, characterized in that: In step 4), during the spinning process, nitrogen gas at 240-260° C. is introduced to volatilize the solvent; In step 4), the heat treatment temperature is 320-360° C. and the heat treatment time is 1-3 h; In step 4), the stretching ratio is 1.0-2.0 times, and the stretching temperature is 420-460°C.
9. The basalt insulating composite material according to claim 1, characterized in that: In step 5), the mass ratio of epoxy resin to modified fiber is 100:(30-45); In step 5), the amount of curing agent added is 30%-50% of the mass of the epoxy resin; The epoxy resin is selected from epoxy resin E51, and the curing agent is selected from epoxy resin curing agent T31; The heating and curing step in step 5) includes first curing at 120-150° C. for 3-8 hours, then cooling to 80-90° C. and continuing curing for 10-20 hours.
10. Use of the basalt insulating composite material according to any one of claims 1 to 9 in an operating rod.
Citation Information
Patent Citations
Fiber, yarn, fabric and product prepared from sulfonyl-containing aromatic polymer and preparation method thereof
CN104846468A
Preparation method of self-repairing insulated operation rod for electrician operation
CN112428598A