Mussel bionic temperature-resistant and salt-resistant thickener and preparation method thereof, and gel fracturing fluid and preparation method thereof and application thereof

Through mussel bionic temperature-resistant, salt-resistant thickener and RAFT controlled polymerization technology, a frozen gel fracturing liquid with a non-covalent-covalent multipolymer network structure was developed, solving the limited temperature resistance and high cost in the existing technology The problem of this has achieved efficient ultra-deep oil and gas development.

CN117659273BActive Publication Date: 2024-11-12CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311641979.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2024-11-12
Estimated Expiration
2043-12-01

AI Technical Summary

Technical Problem

The existing frozen glue fracturing fluid has limited temperature resistance in ultra-deep oil and gas reservoirs, and the synthetic polymer thickener structure is complex, resulting in high production costs and poor quality stability, making it difficult to meet the demand for ultra-high temperature ultra-deep fracturing.

Method used

Using mussel bionic temperature-resistant and salt-resistant thickener, quaternary copolymers are synthesized by RAFT controlled polymerization method, combined with non-covalent-covalent multipolymer network structure, forming supramolecular-enhanced frozen gel fracturing fluid, which has excellent temperature resistance, salt resistance and shear recovery performance.

Benefits of technology

The viscosity of 85.7mPa·s was retained at 200°C for 2h at 170s-1, and the recovery rate after destructive shear reached 92.1%. It is suitable for deep/ultra-deep oil and gas development, reducing production costs and improving Quality stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117659273B_ABST
    Figure CN117659273B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of deep / ultra-deep oil and gas reservoir fracturing fluid, and discloses a mussel bionic temperature-resistant and salt-resistant thickener and a preparation method thereof, and a gel fracturing fluid and a preparation method and application thereof. The thickener contains structural units shown in formulas (a) to (f); m is 52-63, x is 2-7, y is 4-12, and z is 8-16; the gel fracturing fluid has a covalent-non-covalent multiple polymer network, and has excellent temperature resistance, salt resistance, and shear recovery; #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of deep / ultra-deep oil and gas reservoir fracturing fluid, and in particular to a mussel bionic temperature-resistant and salt-resistant thickener and a preparation method thereof, and a gel fracturing fluid and a preparation method and application thereof. Background Art

[0002] As the exploration and development level continues to deepen, oil and gas exploration and development has developed from medium and shallow layers to deep and ultra-deep layers. Deep / ultra-deep oil and gas resources are the key breakthrough areas for my country's future oil and gas exploration and development and reserve and production increase. Fracturing is an important means to achieve efficient development of ultra-deep oil and gas, but the ultra-high temperature conditions faced by ultra-deep fracturing pose new challenges to fracturing fluids. Ultra-deep fracturing development is accompanied by ultra-high temperature and harsh conditions, which puts higher requirements on the performance of fracturing fluids. The use of gel fracturing fluids with a spatial network structure is the most commonly used method to improve the temperature and shear resistance of fracturing fluids. Thickeners are one of the key materials for gel fracturing fluids. Their main function is to maintain the viscosity of the fracturing fluid system under working conditions and to give the system a certain wellbore drag reduction and reservoir sand carrying capacity. Conventional fracturing fluid thickeners are easily decomposed and destroyed under high temperature conditions, causing the system to lose stability and the viscosity to drop rapidly, which does not meet the technical requirements of fracturing construction.

[0003] At present, the commonly used high-temperature resistant thickeners for water-based fracturing fluids at home and abroad mainly include guar gum and its derivatives, viscoelastic surfactants and synthetic polymers.

[0004] Guar gum and its derivatives: CN112111264B discloses a guar gum graft copolymer nano-composite gel fracturing fluid and its preparation method, the fracturing fluid comprises the following components in percentage by weight: 0.4-1.2% guar gum graft copolymer thickener, 0.05-0.5% nanomaterial and 0.2-1% crosslinker, the balance being water; the guar gum graft copolymer thickener is synthesized from the following components in parts by weight: 2-10 parts of guar gum or guar gum derivatives, 5-25 parts of acrylamide monomers, 0.1-2 parts of initiator and 800-1500 parts of water, a hydrophilic flexible polymer side chain is introduced into the semi-rigid macromolecular chain of guar gum, which is then used as a thickener, a nanomaterial dispersion is added, and a nano-composite gel fracturing fluid is prepared under the action of a crosslinker. The fracturing fluid is 170s -1, sheared at 160°C for 2h, the retained viscosity is less than 100mPa·s. CN108018035B discloses a shear-resistant low-concentration guar zirconium jelly fracturing fluid, which comprises the following components in percentage by mass: 0.2-0.6% carboxymethyl hydroxypropyl guar gum, 0.1-0.4% clay stabilizer, 0.2-0.4% drainage aid, 0.2-0.4% cross-linking agent, 0.1-0.3% rheology regulator, pH regulator and water; the cross-linking agent is selected from an organic zirconium cross-linking agent or a water-based zirconium cross-linking agent, and the organic zirconium cross-linking agent is selected from tetra(n-propyl) zirconate, tetra(triethanolamine) zirconate, tetralactic zirconate, and lactic acid tri(triethanolamine) zirconate; the water-based zirconium cross-linking agent is a complex formed by the reaction of an inorganic zirconium salt and a hydroxycarboxylate; the guar zirconium jelly fracturing fluid is resistant to shearing at 160°C and 170s -1 Under the conditions of shearing for 90 minutes, the apparent viscosity of the system is 124mPa·s. The modified guar gum does improve the temperature resistance of guar gum fracturing fluid and broaden the application range of guar gum fracturing fluid, but it is limited by the temperature resistance limit of the glycosidic bond in the guar gum polymer chain (it will be degraded if it exceeds 177℃), so the upper limit of the use temperature of guar gum fracturing fluid is 180-200℃.

[0005] Viscoelastic surfactant: Viscoelastic surfactant fracturing fluid forms micelles through strong interaction between viscoelastic surfactant and counterion, so that the system has excellent viscoelastic properties and sand carrying performance. CN114805115A discloses a heat-resistant dihydroxy cationic viscoelastic surfactant and its preparation method, fracturing fluid and its application. The clean fracturing fluid with a heat-resistant dihydroxy cationic viscoelastic surfactant as a thickener has a high viscosity at 220°C and 170s when the surfactant is added at 5wt%. -1 After shearing for 2 hours under the same conditions, the viscosity is maintained at 30mPa·s. CN113600095A discloses a β-CD Gemini viscoelastic surfactant and its preparation method and a temperature-resistant and salt-resistant clean fracturing fluid. The clean fracturing fluid prepared with 3% thickener + 3% NaSal is heated to 120°C and 170s -1 The system retains viscosity of about 100 mPa·s after 90 min shearing under the above conditions. The existing methods to improve the temperature resistance of surfactant fracturing fluids are mainly through the research and development of complex viscoelastic surfactants, most of which can only be applied to medium and high temperature reservoirs, and generally have problems such as difficulty in industrial production, large amount of thickener, and high cost.

[0006] In terms of synthetic polymers: the CC bond energy contained in synthetic polymers is larger, and the molecular chain is not easy to break under high temperature conditions. At present, the main copolymers used in high-temperature reservoir hydraulic fracturing are polyacrylamide-based copolymers, which have excellent performance in thickening, gel breaking, temperature resistance and reducing residue damage. CN115074106B discloses a gel fracturing fluid and a preparation method thereof, wherein the gel fracturing fluid comprises a thickener, a crosslinker and water, wherein the thickener comprises acrylamide, a sulfonic acid monomer, a promoting monomer, a reinforcing monomer, and 1-isopropenyl-2-benzimidazolone, wherein the promoting monomer is vinyl tri(dimethylsiloxy) silane and / or allyloxy-tert-butyl-dimethylsilane, and the reinforcing monomer is 2-(diisopropylamino) ethyl methacrylate and / or 2-carbonyl-tetrahydrofuran-3-hydroxy-methylacrylate. The thickener is a five-membered copolymer, or even a seven-membered copolymer, and the structure is too complicated. CN114621743A discloses a slow cross-linking temperature-resistant and salt-resistant polymer gel fracturing fluid and its preparation method and application. The fracturing fluid comprises a polymer thickener, a cross-linking agent, a gel breaker, a drainage agent, a clay stabilizer and water. The thickener is a tetrapolymer synthesized from acrylamide, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and vinylimidazole. The thickener is added in an amount of 0.6% and the viscosity is 170s. -1 , sheared at 160℃ for 2h, the retained viscosity was about 50mPa·s.

[0007] Gel fracturing fluid with synthetic multi-polymer as thickener is the main method to deal with ultra-high temperature reservoir fracturing at home and abroad. It mainly relies on high-concentration thickeners and cross-linking agents to construct high-strength gel to cope with ultra-high temperature challenges, which brings about problems such as difficulty in breaking gel, low return rate, high reservoir damage and difficult cost control.

[0008] The research and development of ultra-high temperature resistant thickeners is a fundamental issue for achieving efficient development of ultra-deep oil and gas reservoirs. In order to meet the requirements of ultra-deep fracturing fluids for heat and shear resistance, synthetic polymers are usually designed as complex molecular structures of multifunctional multifunctional monomers, such as five-membered or even seven-membered copolymers. The complex molecular structure is not conducive to the industrial scale-up production of thickeners, resulting in low thickener yield, high cost and poor quality stability. Summary of the invention

[0009] The purpose of the present invention is to overcome the problems of limited temperature resistance and complex structure of synthetic polymer thickeners in the existing gel fracturing fluids used in ultra-deep oil and gas reservoir fracturing, and to provide a mussel bionic temperature-resistant and salt-resistant thickener and a preparation method thereof, a gel fracturing fluid and a preparation method and application thereof. The gel fracturing fluid has a covalent-non-covalent multiple polymer network and has excellent temperature resistance, salt resistance and shear recovery.

[0010] In order to achieve the above-mentioned object, the present invention provides a mussel biomimetic temperature-resistant and salt-resistant thickener on one hand, wherein the thickener contains structural units represented by formula (a) to formula (f);

[0011]

[0012] Among them, m is 52-63, x is 2-7, y is 4-12, and z is 8-16.

[0013] The second aspect of the present invention provides a method for preparing a mussel biomimetic temperature-resistant and salt-resistant thickener, wherein the preparation method comprises:

[0014] (1) in the presence of a xanthate-based water-soluble macromolecular chain transfer agent, contacting acrylamide, sodium acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 3-acrylamido dopamine and water to perform a reversible addition-fragmentation chain transfer polymerization reaction to obtain a first reaction system;

[0015] (2) contacting the first reaction system with an initiator under water bath conditions to carry out heating reaction to obtain a second reaction system;

[0016] (3) The second reaction system is cleaned and vacuum dried to obtain a mussel biomimetic temperature-resistant and salt-resistant thickener.

[0017] The third aspect of the present invention provides a mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the aforementioned preparation method.

[0018] A fourth aspect of the present invention provides a method for preparing a gel fracturing fluid, wherein the preparation method comprises:

[0019] S201: contacting a mussel bionic heat-resistant and salt-resistant thickener with water to obtain a reaction system S201; wherein the mussel bionic heat-resistant and salt-resistant thickener is the mussel bionic heat-resistant and salt-resistant thickener described above;

[0020] S202: Under stirring conditions, the reaction system S201 is contacted with a cross-linking agent to perform dissolution and aging reactions to obtain a gel fracturing fluid.

[0021] A fifth aspect of the present invention provides a gel fracturing fluid prepared by the aforementioned preparation method.

[0022] A sixth aspect of the present invention provides an application of the aforementioned gel fracturing fluid in the fracturing development of deep / ultra-deep oil and gas reservoirs.

[0023] Through the above technical solution, the beneficial effects of the present invention are:

[0024] (1) The mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the present invention is a quaternary copolymer of mussel biomimetic catechol monomers (3-acrylamidopamine), sulfonate monomers, acrylamide, and sodium acrylate. The RAFT controlled polymerization method is adopted, the polymerization reaction conditions are mild, and the product properties are stable.

[0025] (2) Mussel-inspired catechol monomers contain abundant phenolic hydroxyl groups and ring groups, which can realize multiple non-covalent supramolecular interactions including π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling. The highly polar sulfonic acid group can improve the tolerance of the polymer to salt concentration in water. Acrylamide and sodium acrylate provide abundant cross-linking groups (amide and carboxyl groups), which can be chemically cross-linked with transition non-metal cross-linkers (borax, organic boron), transition metal cross-linkers (chromium trichloride, titanium tetrachloride, zirconium oxychloride, organic zirconium, organic titanium, etc.), and polymer cross-linkers (polyethyleneimine, phenolic resins). With abundant cross-linking groups, the cross-linking agent can be selected according to the needs of different development methods to achieve rapid gelation in a wide temperature range. The prepared supramolecular reinforced gel can be extended to various actual oilfield development applications and has great application potential in high-temperature reservoir fracturing, gel water plugging / gas sealing, and foam stabilization.

[0026] (3) The method for preparing supramolecular action enhanced gel fracturing fluid proposed in the present invention has a non-covalent-covalent composite network structure. Among them, mussel biomimetic catechol monomers provide multiple supramolecular actions to construct a non-covalent polymer network, and acrylamide monomers and sodium acrylate monomers provide amide and carboxyl cross-linking sites, which are chemically cross-linked with cross-linking agents to form a covalent polymer network structure. Two types of polymer network structures exist simultaneously in the constructed supramolecular action enhanced gel fracturing fluid, which has advantages in temperature resistance, shear resistance, and salt resistance compared with the gel fracturing fluid prepared by single chemical cross-linking. Zirconium gel fracturing fluid prepared with tap water and 0.6% thickener, 170s -1 After shearing at 200℃ for 2h, the retained viscosity is about 85.7mPa·s, and the viscosity recovery rate after shearing reaches 92.1%.

[0027] (4) The supramolecular action enhanced gel fracturing fluid of the present invention is suitable for deep / ultra-deep oil and gas development, and provides solutions and reference ideas for further improving the fracturing working fluid technology for efficient development of deep / ultra-deep oil and gas in my country. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart of the preparation method of the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) provided by the present invention;

[0029] Figure 2This is a flow chart of the preparation method of the supramolecular action enhanced gel fracturing fluid provided by the present invention;

[0030] Figure 3 This is a schematic diagram of the covalent-non-covalent composite polymer network of the supramolecular action enhanced gel fracturing fluid provided by the present invention;

[0031] Figure 4 The supermolecular effect of the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) provided in Example 4 of the present invention and the organic zirconium to strengthen the gel fracturing fluid at 200°C and 170s -1 The shear viscosity changes with time at a shear rate of;

[0032] Figure 5 The large strain cyclic shear curve of the supramolecular effect-enhanced gel fracturing fluid formed by the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) and organic zirconium provided in Example 4 of the present invention;

[0033] Figure 6 The supermolecular effect of the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) provided in Example 5 of the present invention and the phenolic resin to strengthen the gel fracturing fluid at 200°C and 170s -1 The shear viscosity changes with time at a shear rate of;

[0034] Figure 7 The supermolecular effect of the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) and polyethyleneimine provided in Example 6 of the present invention is used to strengthen the gel fracturing fluid at 200°C and 170s -1 The shear viscosity changes with time at a shear rate of;

[0035] Figure 8 This is the large strain cyclic shear curve of the zirconium jelly fracturing fluid formed by the thickener (without mussel biomimetic monomer) (p[AM-AANa-AMPS]) provided in Comparative Example 3 of the present invention and organic zirconium. DETAILED DESCRIPTION

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] As mentioned above, the first aspect of the present invention provides a mussel biomimetic temperature-resistant and salt-resistant thickener, wherein the thickener contains structural units represented by formula (a) to formula (f);

[0038]

[0039] Among them, m is 52-63, x is 2-7, y is 4-12, and z is 8-16.

[0040] According to the present invention, preferably, m is 58-63, x is 4-7, y is 5-10, and z is 8-10; more preferably, m is 60-63, x is 4-7, y is 6-10, and z is 8-10.

[0041] According to the present invention, preferably, the thickener has a structure as shown in formula (1);

[0042]

[0043] The inventors of the present invention have found that: based on the idea of ​​mussel bionics, a mussel bionic temperature-resistant and salt-resistant thickener suitable for deep / ultra-deep oil and gas fracturing development is proposed. The main process is: using acrylic anhydride and dopamine hydrochloride (DOPA) as reaction raw materials, synthesizing mussel bionic catechol monomers (3-acrylamido dopamine, AM-DOPA) containing both an addible vinyl group and a mussel bionic catechol (catechol) group; using methyl 2-bromopropionate, potassium ethyl xanthate and acrylamide as reaction raw materials, and the initiator is 4,4'-azobis(4-cyanovaleric acid) ), synthesize xanthate water-soluble macromolecular chain transfer agent (PAM-X) for reversible addition-fragmentation chain transfer polymerization (RAFT); acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) are used as reaction raw materials, the chain transfer agent is a synthetic water-soluble xanthate lipid (PAM-X), and the initiator is azobisisobutylamidine hydrochloride (AIBA), and a mussel biomimetic temperature-resistant and salt-resistant thickener is synthesized by RAFT active / controllable polymerization method. The byssus protein secreted by the simulated marine organism mussel can firmly adhere to the rock surface in a seawater environment, and its byssus also has excellent self-repairing properties. The mussel biomimetic catechol monomers provided by the present invention provide multiple supramolecular effects to construct a non-covalent polymer network, and the amide and carboxyl cross-linking sites provided by the acrylamide monomer and the sodium acrylate monomer form a covalent polymer network structure through chemical cross-linking with a cross-linking agent. Therefore, the supramolecular action enhanced gel fracturing fluid prepared by the present invention has a non-covalent-covalent composite network structure.

[0044] Furthermore, the inventors of the present invention have found that the thickener is characterized by containing mussel biomimetic catechol monomers, sulfonate monomers, acrylamide, and sodium acrylate tetrapolymer. The byssus protein secreted by the marine organism mussel can firmly adhere to the rock surface in the seawater environment, and its byssus also has excellent self-repairing properties, which is mainly attributed to the multiple supramolecular effects of the catechol-like structure.

[0045] Furthermore, the inventors of the present invention have found that the mussel biomimetic catechol monomers contain abundant phenolic hydroxyl groups and cyclic groups, which can realize multiple non-covalent supramolecular effects including π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling, so that the polymer chain can form a non-covalent polymer network structure without a cross-linking agent through the above non-covalent effects. Sulfonate monomers are branched anionic side groups with a certain rigid structure that can effectively prevent the chain curling behavior of the polymer at high temperature. At the same time, they contain highly polar sulfonic acid groups, which can improve the tolerance of the polymer to salt concentration in water. Acrylamide is used as a main chain thickening monomer and provides an amide group at the cross-linking site. Sodium acrylate easily forms anionic sodium acrylate in aqueous solution, which can increase the water solubility of the polymer and provide a carboxyl group at the cross-linking site.

[0046] Furthermore, the inventors of the present invention found that the mussel bionic temperature-resistant and salt-resistant thickener contains a large number of cross-linking site amide groups and carboxyl groups, which can be chemically cross-linked with transition non-metal cross-linking agents (borax, organic boron), transition metal cross-linking agents (chromium trichloride, titanium tetrachloride, zirconium oxychloride, organic zirconium, organic titanium, etc.), and polymer cross-linking agents (polyethyleneimine, phenolic resins) to form a covalent polymer network structure.

[0047] According to the present invention, the non-covalent supramolecular force provided by the mussel bionic catechol monomer in the mussel bionic temperature-resistant and salt-resistant thickener provided by the present invention is as follows:

[0048]

[0049] Among them, as mentioned above, mussel biomimetic catechol monomers contain abundant phenolic hydroxyl groups and ring groups, which can realize multiple non-covalent supramolecular effects including π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling, so that the polymer chain can form a non-covalent polymer network structure without a crosslinking agent through the above non-covalent effects. Sulfonate monomers are 2-acrylamido-2-methylpropanesulfonic acid as branched anionic side groups, which have a certain rigid structure that can effectively prevent the chain curling behavior of the polymer at high temperature. At the same time, they contain highly polar sulfonic acid groups, which can improve the tolerance of the polymer to salt concentration in water. Acrylamide is used as a main chain thickening monomer and provides an amide group at the crosslinking site. Sodium acrylate easily forms anionic sodium acrylate in aqueous solution, which can increase the water solubility of the polymer and provide a carboxyl group at the crosslinking site.

[0050] The second aspect of the present invention provides a method for preparing a mussel biomimetic temperature-resistant and salt-resistant thickener, wherein the preparation method comprises:

[0051] (1) in the presence of a xanthate-based water-soluble macromolecular chain transfer agent, contacting acrylamide, sodium acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 3-acrylamido dopamine and water to perform a reversible addition-fragmentation chain transfer polymerization reaction to obtain a first reaction system;

[0052] (2) contacting the first reaction system with an initiator under water bath conditions to carry out heating reaction to obtain a second reaction system;

[0053] (3) The second reaction system is cleaned and vacuum dried to obtain a mussel biomimetic temperature-resistant and salt-resistant thickener.

[0054] The inventors of the present invention have found that mussel biomimetic catechol monomers (AM-DOPA) provide multiple supramolecular effects to construct a non-covalent polymer network, and acrylamide monomers (AM) and sodium acrylate monomers (AANa) provide amide and carboxyl crosslinking sites, which can form a covalent polymer network structure by chemical crosslinking with a crosslinking agent. The two types of polymer network structures exist simultaneously in the constructed supramolecular effect-enhanced gel fracturing fluid, which has advantages in temperature resistance, shear resistance, and salt resistance compared to gel fracturing fluids prepared by single chemical crosslinking.

[0055] In the present invention, acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), and 2-acrylamide-2-methylpropanesulfonic acid (AMPS) are used as reaction raw materials, a chain transfer agent is a synthetic water-soluble xanthate (PAM-X), and an initiator is azobisisobutylamidine hydrochloride (AIBA), and a mussel biomimetic temperature-resistant and salt-resistant thickener is synthesized through a RAFT active / controllable polymerization method.

[0056] According to the present invention, the RAFT active / controllable polymerization method is applicable to a wide range of monomers, especially acrylamide monomers; the use of heavy metal catalysts can be avoided to reduce pollution; the polymerization reaction conditions are mild and meet the commonly used temperature range; the chain transfer agent is an important regulator in the RAFT active / controllable polymerization, and the commonly used types are: dithioesters, trithiocarbonates, dithiocarbamates, xanthates, etc.; preferably, xanthates have low odor, low toxicity, simple synthesis method, and wide monomer adaptability; more preferably, a xanthate chain transfer agent (PAM-X) is selected.

[0057] According to the present invention, in step (1), the sodium acrylate is sodium acrylate and / or potassium acrylate, preferably sodium acrylate (AANa). In the present invention, acrylic acid and sodium hydroxide solution can be prepared into a sodium acrylate (AANa) aqueous solution.

[0058] According to the present invention, in step (1), acrylamide (AM), sodium acrylate aqueous solution, 3-acrylamidopamine (AM-DOPA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and chain transfer agent (PAM-X) are added to an aqueous solution according to a certain molar ratio, magnetically stirred for dissolution, and nitrogen is introduced for deoxygenation for 30-60 minutes to obtain a first reaction system; wherein, in the first reaction system, the concentration of the monomer solution is 30-40% by weight.

[0059] According to the present invention, the molar ratio of acrylamide (AM), sodium acrylate, 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 3-acrylamido dopamine (AM-DOPA) is (63-75):(3-8):(5-15):(10-20), preferably (65-73):(5-8):(5-15):(15-20).

[0060] According to the present invention, the mass ratio of the chain transfer agent to the initiator is (0.05-0.2): (0.3-0.5);

[0061] According to the present invention, in step (2), an initiator is added to the first reaction system, and the reaction is heated in a water bath to obtain a second reaction system; wherein the initiator is azobisisobutyramidine hydrochloride (AIBA).

[0062] According to the present invention, in step (2), the conditions for water bath heating include: temperature of 45-60° C. and time of 4-6 h.

[0063] According to the present invention, in step (3), the vacuum drying temperature is 50-60°C, preferably, the vacuum drying temperature is 50°C.

[0064] According to the present invention, the mussel biomimetic catechol monomer 3-acrylamide dopamine (AM-DOPA) can be obtained by self-production. In the present invention, the preparation method of the 3-acrylamide dopamine (AM-DOPA) comprises:

[0065] (a) contacting and dissolving sodium tetraborate decahydrate with methanol to obtain a reaction system a;

[0066] (b) under nitrogen protection, contacting dopamine hydrochloride with the reaction system a, and after the dopamine hydrochloride is completely dissolved, adjusting the solution to a weak alkalinity with sodium carbonate to obtain a reaction system b;

[0067] (c) adding acrylic anhydride dropwise to the reaction system b to react, and after the reaction is completed, adjusting the solution to acidity with hydrochloric acid to obtain a reaction system c;

[0068] (d) subjecting the reaction system c to vacuum rotary evaporation to remove the solvent, and then subjecting the reaction system c to vacuum oven drying to obtain 3-acrylamide dopamine.

[0069] According to the present invention, the molar ratio of sodium tetraborate decahydrate, dopamine hydrochloride and acrylic anhydride is (2-4): (2-4): (1-2).

[0070] According to the present invention, in step (a), sodium tetraborate decahydrate is dissolved in methanol and magnetically stirred for 20-40 minutes in a nitrogen atmosphere to fully dissolve it, thereby obtaining a reaction system a.

[0071] According to the present invention, in step (b), nitrogen is continuously introduced, dopamine hydrochloride is added to the first reaction system, and after the dopamine hydrochloride is completely dissolved under continuous magnetic stirring, the solution is adjusted to weak alkalinity with sodium carbonate, and the pH of the weak alkalinity is 9.5-10.5, to obtain reaction system b. In addition, dopamine hydrochloride provides a key functional group of mussel biomimetic: catechol structure, and the chemical structure is as follows:

[0072]

[0073] According to the present invention, in step (c), nitrogen is continuously introduced, acrylic anhydride is slowly dripped into the second reaction system, and the reaction is carried out for 12-24 hours under continuous weak magnetic stirring. After the reaction, the solution is adjusted to acidity with hydrochloric acid to obtain a reaction system c; wherein the reaction temperature is 20-35°C; and the acidic pH is 1.5-2.

[0074] According to the present invention, in step (d), the reaction system c is subjected to vacuum rotary evaporation to remove the solvent, and then subjected to vacuum oven drying treatment to obtain a mussel bionic catechol monomer (3-acrylamide dopamine, AM-DOPA) containing both an addable vinyl group and a mussel bionic catechol (catechol) group.

[0075] In the present invention, the vacuum rotary evaporation temperature is 50-60°C, preferably 50°C; the vacuum oven drying temperature is 50-60°C, preferably 50°C.

[0076] According to the present invention, the chain transfer agent has the general formula shown in formula (2):

[0077]

[0078] Among them, n is 5-10.

[0079] According to the present invention, the chain transfer agent is a synthetic water-soluble xanthate (PAM-X), which can be obtained by self-production. In the present invention, the preparation method of the chain transfer agent (PAM-X) comprises:

[0080] (e) contacting methyl 2-bromopropionate with methanol to dissolve the mixture and then cooling the mixture in an ice-water bath to obtain a reaction system e;

[0081] (f) contacting the reaction system e with potassium ethyl xanthate to react to obtain a reaction system f;

[0082] (g) removing the solvent from the reaction system f by vacuum rotary evaporation and then drying in a vacuum oven to obtain an intermediate product X;

[0083] (h) contacting the intermediate product X, acrylamide, ethanol, and water under nitrogen protection to obtain a reaction system h;

[0084] (i) contacting the reaction system h with an initiator under water bath conditions to carry out heating reaction to obtain a reaction system i;

[0085] (j) subjecting the reaction system i to vacuum rotary evaporation to remove the solvent and then subjecting the reaction system i to vacuum oven drying to obtain a chain transfer agent.

[0086] In the present invention, methyl 2-bromopropionate, potassium ethyl xanthate and acrylamide are used as reaction raw materials and 4,4'-azobis(4-cyanovaleric acid) is used as initiator to synthesize a xanthate-based water-soluble macromolecular chain transfer agent (PAM-X) for reversible addition-fragmentation chain transfer polymerization (RAFT).

[0087] According to the present invention, in step (e), methyl 2-bromopropionate is dissolved in methanol by magnetic stirring, and the flask containing the solution is placed in an ice-water bath for cooling to obtain a reaction system e; wherein the molar ratio of methyl 2-bromopropionate and potassium ethyl xanthate is (4-6):(5-7); and the temperature of the ice-water bath is -6°C to -2°C.

[0088] According to the present invention, in step (f), potassium ethyl xanthate is slowly added to the reaction system e. After the addition is completed, the reaction is carried out at a temperature of 25-30° C. for 12-20 hours. The reaction is completed to obtain a reaction system f.

[0089] According to the present invention, in step (g), the reaction system f is subjected to vacuum rotary evaporation to remove the solvent, and then subjected to vacuum oven drying treatment to obtain an intermediate product X; wherein the molar ratio of the intermediate product X to acrylamide is (1-2):(5-10).

[0090] According to the present invention, in step (h), the intermediate product X and acrylamide are added to ethanol / water (volume ratio 1:1), and nitrogen is introduced for deoxygenation for 30-60 minutes to obtain a reaction system h.

[0091] According to the present invention, in step (i), an initiator 4,4'-azobis(4-cyanovaleric acid) is added to the reaction system h, and the reaction is heated in a water bath to obtain a reaction system i; wherein the initiator is 4,4'-azobis(4-cyanovaleric acid); and the amount of the initiator used is 0.05-0.2% by weight based on the total weight of methyl 2-bromopropionate and potassium ethyl xanthate.

[0092] According to the present invention, in step (i), the reaction temperature is 50-70° C. and the reaction time is 2-4 hours.

[0093] According to the present invention, in step (j), the reaction system i is subjected to vacuum rotary evaporation to remove the solvent, and then subjected to vacuum oven drying treatment to obtain a xanthate-based water-soluble macromolecular chain transfer agent (PAM-X). In the present invention, the vacuum rotary evaporation temperature is 50-60°C, preferably 50°C; the vacuum oven drying temperature is 50-60°C, preferably 50°C.

[0094] According to a preferred embodiment of the present invention, the synthesis route of the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) provided by the present invention is as follows:

[0095] ①Mussel biomimetic catechol monomer (3-acrylamidopamine, AM-DOPA)

[0096]

[0097] ②Xanthate water-soluble macromolecular chain transfer agent (PAM-X)

[0098]

[0099] ③Mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS])

[0100]

[0101] It should be noted that the acrylamide in step ② is the acrylamide in PAM-X, which has a lower content and is used for chain transfer and termination; it is not the acrylamide main chain in the copolymer.

[0102] Figure 1The present invention provides a flow chart of a preparation method of a mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]). Specifically, the preparation method comprises:

[0103] S101: Using acrylic anhydride and dopamine hydrochloride (DOPA) as reaction raw materials, a mussel biomimetic catechol monomer (3-acrylamidopamine, AM-DOPA) containing both an addable vinyl group and a mussel biomimetic catechol (catechol) group was synthesized;

[0104] S102: Using methyl 2-bromopropionate, potassium ethyl xanthate and acrylamide as the reaction raw materials and 4,4'-azobis(4-cyanovaleric acid) as the initiator, a xanthate-based water-soluble macromolecular chain transfer agent (PAM-X) for reversible addition-fragmentation chain transfer polymerization (RAFT) was synthesized;

[0105] S103: Using acrylamide (AM), sodium acrylate (AANa), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 3-acrylamido dopamine (AM-DOPA) as polymerization reaction monomer raw materials, a mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) was synthesized by RAFT active / controllable polymerization method.

[0106] The third aspect of the present invention provides a mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the aforementioned preparation method.

[0107] A fourth aspect of the present invention provides a method for preparing a gel fracturing fluid. Figure 2 : is a flow chart of a method for preparing a supramolecular action enhanced gel fracturing fluid provided by an embodiment of the present invention; wherein the preparation method comprises:

[0108] S201: contacting a mussel bionic heat-resistant and salt-resistant thickener with water to obtain a reaction system S201; wherein the mussel bionic heat-resistant and salt-resistant thickener is the mussel bionic heat-resistant and salt-resistant thickener described above;

[0109] S202: Under stirring conditions, the reaction system S201 is contacted with a cross-linking agent to perform dissolution and aging reactions to obtain a gel fracturing fluid.

[0110] According to the present invention, the gel fracturing fluid has a non-covalent-covalent multi-crosslinked polymer composite network structure.

[0111] Specifically, the first type of polymer network structure in the multiple cross-linked polymer composite network structure is based on the mussel bionic catechol monomer (AM-DOPA) in the mussel bionic temperature-resistant and salt-resistant thickener, and through multiple non-covalent supramolecular effects such as π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling, the thickener chain can form a non-covalent polymer network structure through the above non-covalent effects in the absence of a cross-linking agent.

[0112] Specifically, the second type of polymer network structure in the multiple cross-linked polymer composite network structure is based on the amide and carboxyl cross-linking sites provided by acrylamide monomers and sodium acrylate monomers in the mussel bionic heat-resistant and salt-resistant thickener, and is chemically cross-linked with a cross-linking agent to form a covalent polymer network structure.

[0113] Specifically, the two types of polymer network structures exist simultaneously in the constructed supramolecular action enhanced gel fracturing fluid.

[0114] Figure 3 Schematic diagram of the covalent-non-covalent composite polymer network of the supramolecular action enhanced gel fracturing fluid provided by the present invention; Figure 3 It can be seen that the first type of polymer network structure in the multiple cross-linked polymer composite network structure is based on the mussel bionic catechol monomer (AM-DOPA) in the mussel bionic heat-resistant and salt-resistant thickener, and through multiple non-covalent supramolecular effects such as π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling, the thickener chain can form a non-covalent polymer network structure through the above non-covalent action without a cross-linking agent; at the same time, the second type of polymer network structure in the multiple cross-linked polymer composite network structure is based on the amide and carboxyl cross-linking sites provided by acrylamide monomers and sodium acrylate monomers in the mussel bionic heat-resistant and salt-resistant thickener, and forms a covalent polymer network structure through chemical cross-linking with a cross-linking agent. It should be noted that the two types of polymer network structures exist simultaneously in the constructed supramolecular action-enhanced gel fracturing fluid.

[0115] According to the present invention, the crosslinking agent is selected from one or more of organic zirconium, organic titanium, borax, organic boron, phenolic resin and polyethylene imine; preferably, the crosslinking agent is selected from one or more of organic zirconium, phenolic resin and polyethylene imine.

[0116] According to the present invention, the mussel bionic temperature-resistant and salt-resistant thickener provided by the present invention is cross-linked with organic zirconium to form a bond, as shown below:

[0117]

[0118] According to the present invention, the mass ratio of the organic zirconium to water is (5-16): (984-995).

[0119] According to the present invention, when the cross-linking agent is organic zirconium, the reaction temperature is 65-80°C.

[0120] According to the present invention, the mussel bionic temperature-resistant and salt-resistant thickener provided by the present invention is cross-linked with the phenolic resin to form a bond, as shown below:

[0121]

[0122] According to the present invention, the mass ratio of the phenolic resin to water is (15-24): (976-985).

[0123] According to the present invention, when the cross-linking agent is phenolic resin, the reaction temperature is 70-90°C.

[0124] According to the present invention, the mussel biomimetic temperature-resistant and salt-resistant thickener provided by the present invention is cross-linked with polyethyleneimine

[0125] The keys are as follows:

[0126]

[0127] According to the present invention, the mass ratio of the polyethyleneimine to water is (2-10): (990-998).

[0128] According to the present invention, when the cross-linking agent is polyethyleneimine, the reaction temperature is 120-160°C.

[0129] According to the present invention, the mass ratio of the mussel bionic temperature-resistant and salt-resistant thickener to water is (5-8): (992-995).

[0130] A fifth aspect of the present invention provides a gel fracturing fluid prepared by the aforementioned preparation method.

[0131] According to the present invention, the supramolecular action enhanced gel fracturing fluid has multiple polymer network structures, including: the first type of polymer network structure is based on mussel biomimetic catechol monomers (AM-DOPA) in mussel biomimetic heat-resistant and salt-resistant thickeners, through multiple non-covalent supramolecular actions such as π-π stacking, Michael addition, cation-π, hydrogen bonding and Di-DOPA coupling, so that the thickener chain can form a non-covalent polymer network structure through the above non-covalent action without a cross-linking agent; the second type of polymer network structure is based on the amide and carboxyl cross-linking sites provided by acrylamide monomers and sodium acrylate monomers in mussel biomimetic heat-resistant and salt-resistant thickeners, and forms a covalent polymer network structure through chemical cross-linking with a cross-linking agent. It should be noted that the two types of polymer network structures exist simultaneously in the constructed supramolecular action enhanced gel fracturing fluid.

[0132] According to the present invention, the supramolecular action enhanced zirconium gel fracturing fluid prepared with tap water and 0.6% thickener, 170s -1 , sheared at 200℃ for 2h, the retained viscosity was about 85.7mPa·s, and the viscosity recovery rate after destructive shearing reached 92.1%.

[0133] A sixth aspect of the present invention provides an application of the aforementioned gel fracturing fluid in the fracturing development of deep / ultra-deep oil and gas reservoirs.

[0134] The present invention will be described in detail below through examples.

[0135] In the following embodiments:

[0136] The rheological properties of the prepared various types of gel fracturing fluids were measured by a high temperature and high pressure rheometer (HaaKe RS60, Thermo Fisher Scientific (China) Co., Ltd.).

[0137] The specific steps of the temperature and shear resistance test are as follows: according to the performance evaluation method of water-based fracturing fluid in the petroleum and natural gas industry standard of the People's Republic of China (SY / T 5107-2005), the shear rate is set to a constant 170s -1 , the temperature was raised to 200°C, the shear time was 2h, and the viscosity-temperature-time relationship curve was obtained.

[0138] The large strain cyclic shear curve is mainly used to determine the viscosity recovery ability of the gel. The test temperature is set at 25°C and the angular frequency is constant (ω = 6.28 rad·s -1 ), and perform strain sweep test with strain variation range of 1%-5000%. The two modulus curves will intersect and determine the critical failure point (intersection point of G' and G''). Then, take a value before and after the critical failure point to perform multiple cycles of shear strain oscillation sweep, which lasts for 600s under high shear failure strain and 100s under low shear strain. The elastic modulus recovery rate of the gel is calculated to evaluate the viscosity recovery ability of the gel, and indirectly clarify the strength of supramolecular non-covalent interaction.

[0139] In the synthesis process of mussel biomimetic temperature-resistant and salt-resistant thickener, raw materials dopamine hydrochloride (analytical grade, 97%), sodium tetraborate decahydrate (analytical grade, 97%), acrylic anhydride (analytical grade, 98%), methyl 2-bromopropionate (analytical grade, 98%), potassium ethyl xanthate (analytical grade, 98%), acrylamide (analytical grade, 99%), acrylic acid (analytical grade, 99%), 2-acrylamide-2-methylpropanesulfonic acid (analytical grade, 99%), and solvent methanol (analytical grade, 99%) were purchased from Shanghai MacLean Biochemical Technology Co., Ltd., initiators 4,4'-azobis(4-cyanovaleric acid) (analytical grade, 99%) and azobisisobutyramidine hydrochloride (analytical grade, 99%) were purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd., and the water used was laboratory-made deionized water (ULUPURE, UPT-Ⅱ). All reagents were prepared and used immediately without further purification.

[0140] In the process of supramolecular enhancement of frozen gel fracturing fluid, the mussel bionic temperature-resistant and salt-resistant thickener was homemade, water was laboratory tap water, the cross-linking agent organic zirconium was purchased from Shandong Noel Biotechnology Co., Ltd., the cross-linking agent phenolic resin was purchased from Shandong Shida Oilfield Technology Service Co., Ltd., and the cross-linking agent polyethyleneimine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (analytical grade, 99%, MW 600).

[0141] Example 1

[0142] The embodiment of the present invention is to illustrate the mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the preparation method of the present invention.

[0143] first step:

[0144] Preparation of mussel biomimetic temperature-resistant and salt-resistant thickener, such as Figure 1 As shown, a method for preparing a mussel biomimetic temperature-resistant and salt-resistant thickener is provided, which includes a method for synthesizing a mussel biomimetic catechol monomer (AM-DOPA), a method for synthesizing a water-soluble macromolecular chain transfer agent (PAM-X), and a method for synthesizing acrylamide (AM) / sodium acrylate (AANa) / mussel biomimetic catechol monomer (AM-DOPA) / sulfonate monomer (AMPS) quaternary copolymer. The specific synthetic route is as follows:

[0145] The mussel biomimetic catechol monomer (AM-DOPA) is prepared. Specifically, the synthesis method comprises the following steps:

[0146] (a) First, 0.1 mol of sodium tetraborate decahydrate was dissolved in 50 mL of methanol, and the mixture was magnetically stirred and deoxygenated with N2 for 20 min to fully dissolve the mixture, thereby obtaining reaction system a;

[0147] (b) nitrogen is continuously introduced, 0.1 mol of dopamine hydrochloride is added to the reaction system a, and after the dopamine hydrochloride is completely dissolved under continuous magnetic stirring, sodium carbonate is used to adjust the solution to weak alkalinity (pH=10) to obtain a reaction system b;

[0148] (c) nitrogen was continuously introduced, and 0.05 mol of acrylic anhydride was slowly dripped into the reaction system b, and the reaction was carried out for 24 hours under weak magnetic stirring. After the reaction, the solution was adjusted to acidity (pH=2) with hydrochloric acid to obtain a reaction system c.

[0149] (d) subjecting the reaction system c to vacuum rotary evaporation at 50° C. to remove the solvent, and then subjecting the reaction system c to vacuum oven drying at 50° C. to obtain a mussel biomimetic catechol monomer (3-acrylamidopamine, AM-DOPA) containing both an addable vinyl group and a mussel biomimetic catechol (catechol) group.

[0150] Step 2:

[0151] The water-soluble macromolecular chain transfer agent (PAM-X) is prepared. Specifically, the synthesis method comprises the following steps:

[0152] (e) dissolving 0.05 mol of methyl 2-bromopropionate in 30 mL of methanol by magnetic stirring, and cooling the flask containing the solution in an ice-water bath at -5°C to obtain a reaction system e;

[0153] (f) slowly adding 0.06 mol potassium ethyl xanthate to the reaction system e, and after the addition, moving the mixture to 25° C. for reaction for 20 h, and completing the reaction to obtain a reaction system f;

[0154] (g) subjecting the reaction system f to vacuum rotary evaporation at 50° C. to remove the solvent, and then subjecting the reaction system f to vacuum oven drying at 50° C. to obtain an intermediate product X;

[0155] (h) adding 1 mol of the intermediate product X and 8 mol of acrylamide to ethanol / water (volume ratio 1:1), introducing nitrogen to deoxygenate for 40 min, to obtain a reaction system h;

[0156] (i) adding 0.1% mass concentration of initiator 4,4'-azobis(4-cyanovaleric acid) to reaction system h, heating in a water bath at 60° C. for 3 h to obtain reaction system i;

[0157] (j) the reaction system i is subjected to vacuum rotary evaporation at 50° C. to remove the solvent, and then subjected to vacuum oven drying at 50° C. to obtain a xanthate-based water-soluble macromolecular chain transfer agent (PAM-X); wherein the chain transfer agent has a structure shown in formula (2);

[0158]

[0159] Among them, n is 8.

[0160] Step 3:

[0161] A mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]) is prepared. Specifically, the preparation method comprises:

[0162] (1) Acrylic acid and 1.0 mol·L -1 The sodium hydroxide solution is prepared into a sodium acrylate (AANa) aqueous solution;

[0163] (2) acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS), and a chain transfer agent (PAM-X) with a mass concentration of 0.45% were added to an aqueous solution at a molar ratio of AM:AANa:DOPA:AMPS = 73:5:7:15, the solution concentration was 30%, magnetic stirring was used for dissolution, and nitrogen was introduced for deoxygenation for 40 minutes to obtain a first reaction system;

[0164] (3) adding azobisisobutylamidine hydrochloride (AIBA) with a mass concentration of 0.1% to the first reaction system, heating in a water bath at 50° C. for 6 hours to obtain a second reaction system;

[0165] (4) The second reaction system is repeatedly washed with anhydrous ethanol, and then vacuum dried at 50° C. to obtain the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]), which is labeled as S1.

[0166] In addition, the prepared mussel biomimetic temperature-resistant and salt-resistant thickener S1 has the general formula shown in formula (1):

[0167]

[0168] Furthermore, in formula (1), m is 63, x is 7, y is 10, and z is 8.

[0169] Example 2

[0170] The embodiment of the present invention is to illustrate the mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the preparation method of the present invention.

[0171] The mussel bionic temperature-resistant and salt-resistant thickener used in this embodiment is different from the polymer S1 in Example 1 in that the proportion of functional monomers is changed, further increasing the proportion of mussel bionic supramolecular effects, specifically:

[0172] (1) Acrylic acid and 1.0 mol·L -1The sodium hydroxide solution is prepared into a sodium acrylate (AANa) aqueous solution;

[0173] (2) adding acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and a chain transfer agent (PAM-X) with a mass concentration of 0.45% to an aqueous solution at a molar ratio of AM:AANa:DOPA:AMPS = 65:5:15:15, the solution concentration is 30%, magnetic stirring is used for dissolution, and nitrogen is introduced for deoxygenation for 40 minutes to obtain a first reaction system;

[0174] (3) adding azobisisobutylamidine hydrochloride (AIBA) with a mass concentration of 0.1% to the first reaction system, heating in a water bath at 50° C. for 6 hours to obtain a second reaction system;

[0175] (4) The second reaction system is repeatedly washed with anhydrous ethanol, and then vacuum dried at 50° C. to obtain the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]), which is labeled as S2.

[0176] In addition, the prepared mussel biomimetic temperature-resistant and salt-resistant thickener S2 has the general formula shown in formula (1):

[0177]

[0178] Furthermore, in formula (1), m is 60, x is 4, y is 10, and z is 10.

[0179] Example 3

[0180] The embodiment of the present invention is to illustrate the mussel biomimetic temperature-resistant and salt-resistant thickener prepared by the preparation method of the present invention.

[0181] The mussel bionic temperature-resistant and salt-resistant thickener used in this embodiment is different from the polymer S1 in Example 1 in that the proportion of functional monomers is changed to further reduce the proportion of mussel bionic supramolecular effects, specifically:

[0182] (1) Acrylic acid and 1.0 mol·L -1 The sodium hydroxide solution is prepared into a sodium acrylate (AANa) aqueous solution;

[0183] (2) adding acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and a chain transfer agent (PAM-X) with a mass concentration of 0.45% to an aqueous solution at a molar ratio of AM:AANa:DOPA:AMPS = 75:5:5:15, the solution concentration is 30%, magnetic stirring is used for dissolution, and nitrogen is introduced for deoxygenation for 40 minutes to obtain a first reaction system;

[0184] (3) adding azobisisobutylamidine hydrochloride (AIBA) with a mass concentration of 0.1% to the first reaction system, heating in a water bath at 50° C. for 6 hours to obtain a second reaction system;

[0185] (4) The second reaction system is repeatedly washed with anhydrous ethanol, and then vacuum dried at 50° C. to obtain the mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA-AMPS]), which is labeled as S3.

[0186] In addition, the prepared mussel biomimetic temperature-resistant and salt-resistant thickener S3 has the general formula shown in formula (1):

[0187]

[0188] Furthermore, in formula (1), m is 63, x is 4, y is 6, and z is 9.

[0189] Example 4

[0190] The embodiment of the present invention is to illustrate the supramolecular action enhanced gel fracturing fluid prepared by the preparation method of the present invention.

[0191] like Figure 2 As shown, the preparation method of the supramolecular action enhanced gel fracturing fluid includes:

[0192] (1) adding the mussel biomimetic temperature-resistant and salt-resistant thickener S1 prepared in Example 1 with a mass concentration of 0.6% to a certain amount of water, and stirring until the polymer is completely dissolved to obtain a first reaction system;

[0193] (2) Slowly add 0.6% by mass of an organic zirconium crosslinking agent into the first reaction system, stir until the crosslinking agent is fully soluble, and age in an oven at 70° C. to obtain a supramolecular enhanced gel fracturing fluid, which is labeled as Z1.

[0194] like Figure 4 , Figure 5 As shown, the supramolecular effect enhanced zirconium gel fracturing fluid prepared with tap water and 0.6% thickener, 170s -1, sheared at 200℃ for 2h, the retained viscosity was about 85.7mPa·s, and the viscosity recovery rate after destructive shearing reached 92.1%.

[0195] Example 5

[0196] The embodiment of the present invention is to illustrate the supramolecular action enhanced gel fracturing fluid prepared by the preparation method of the present invention.

[0197] The mussel biomimetic temperature-resistant and salt-resistant thickener used in this example is exactly the same as the polymer S1 obtained in Example 1. The preparation method of the supramolecular action enhanced gel fracturing fluid is similar to that in Example 6, except that the cross-linking agent is replaced by "0.6% organic zirconium" with "1.2% phenolic resin" and the reaction temperature is 75°C.

[0198] Specifically, a mussel biomimetic temperature-resistant and salt-resistant thickener with a mass concentration of 0.6% is added to a certain amount of water and stirred until the polymer is completely dissolved to obtain a first reaction system; a phenolic resin cross-linker with a mass fraction of 1.2% is slowly added to the first reaction system and stirred until the cross-linkers are fully miscible, and an oven aging reaction is performed at 75°C to obtain a supramolecular effect enhanced gel fracturing fluid, which is marked as Z2.

[0199] like Figure 6 As shown, the supramolecular effect enhanced phenolic gel fracturing fluid prepared with tap water and 0.6% thickener, 170s -1 , sheared at 200℃ for 2h, the retained viscosity was about 61.1mPa·s.

[0200] Example 6

[0201] The embodiment of the present invention is to illustrate the supramolecular action enhanced gel fracturing fluid prepared by the preparation method of the present invention.

[0202] The mussel biomimetic temperature-resistant and salt-resistant thickener used in this example is exactly the same as the polymer S1 obtained in Example 1. The preparation method of the supramolecular enhanced gel fracturing fluid is similar to that in Example 6, except that the cross-linking agent is replaced by 0.25% polyethyleneimine from 0.6% organic zirconium, and the reaction temperature is 125°C.

[0203] Specifically, a mussel biomimetic temperature-resistant and salt-resistant thickener with a mass concentration of 0.6% is added to a certain amount of water and stirred until the polymer is completely dissolved to obtain a first reaction system; a polyethyleneimine cross-linker with a mass fraction of 1.2% is slowly added to the first reaction system and stirred until the cross-linkers are fully miscible, and an oven aging reaction is performed at 125°C to obtain a supramolecular action enhanced gel fracturing fluid, which is marked as Z3.

[0204] like Figure 7 As shown, the supramolecular effect enhanced polyethyleneimine gel fracturing fluid prepared with tap water and 0.6% thickener, 170s-1 , sheared at 200℃ for 2h, the retained viscosity was about 77.8mPa·s.

[0205] Example 7

[0206] The embodiment of the present invention is to illustrate the supramolecular action enhanced gel fracturing fluid prepared by the preparation method of the present invention.

[0207] The polymer S2 in Example 2 is used as a thickener, and the preparation method of the supramolecular action enhanced gel fracturing fluid is consistent with that of Example 3. The prepared supramolecular action enhanced gel fracturing fluid is marked as Z4.

[0208] Example 8

[0209] The embodiment of the present invention is to illustrate the supramolecular action enhanced gel fracturing fluid prepared by the preparation method of the present invention.

[0210] The polymer S3 in Example 3 is used as a thickener, and the preparation method of the supramolecular effect enhanced gel fracturing fluid is consistent with that in Example 3. The prepared supramolecular effect enhanced gel fracturing fluid is marked as Z5.

[0211] Comparative Example 1

[0212] A mussel biomimetic temperature-resistant and salt-resistant thickener was prepared in the same manner as in Example 1. The difference between this comparative example and the polymer S1 in Example 1 is that the mussel biomimetic catechol monomer was removed, and p[AM-AANa-AMPS] ternary copolymerization was performed; and the molar ratio of AM:AANa:AMPS was modified, specifically:

[0213] (1) Acrylic acid and 1.0 mol·L -1 The sodium hydroxide solution is prepared into a sodium acrylate (AANa) aqueous solution;

[0214] (2) adding acrylamide (AM), sodium acrylate (AANa), 2-acrylamide-2-methylpropanesulfonic acid (AMPS), and a chain transfer agent (PAM-X) with a mass concentration of 0.45% to an aqueous solution at a molar ratio of AM:AANa:AMPS = 80:5:15, the solution concentration is 30%, magnetic stirring is used for dissolution, and nitrogen is introduced for deoxygenation for 40 minutes to obtain a first reaction system;

[0215] (3) adding azobisisobutylamidine hydrochloride (AIBA) with a mass concentration of 0.1% to the first reaction system, heating in a water bath at 50° C. for 6 hours to obtain a second reaction system;

[0216] (4) The second reaction system was repeatedly washed with anhydrous ethanol and dried in 50° C. vacuum to obtain a temperature-resistant and salt-resistant thickener (p[AM-AANa-AMPS]), which was labeled as DS1.

[0217] In addition, the prepared temperature-resistant and salt-resistant thickener DS1 has the general formula shown in formula (3):

[0218]

[0219] Furthermore, in formula (3), m is 63, y is 10, and z is 8.

[0220] Comparative Example 2

[0221] The mussel biomimetic heat-resistant and salt-resistant thickener was prepared in the same manner as in Example 1. The difference between the mussel biomimetic heat-resistant and salt-resistant thickener used in this comparative example and the polymer S1 in Example 1 is that 2-acrylamide-2-methylpropanesulfonic acid was removed, and p[AM-AANa-DOPA] ternary copolymerization was performed; and the molar ratio of AM:AANa:DOPA was modified, specifically:

[0222] (1) Acrylic acid and 1.0 mol·L -1 The sodium hydroxide solution is prepared into a sodium acrylate (AANa) aqueous solution;

[0223] (2) acrylamide (AM), sodium acrylate (AANa), 3-acrylamidopamine (AM-DOPA), and a chain transfer agent (PAM-X) with a mass concentration of 0.45% were added to an aqueous solution at a molar ratio of AM:AANa:DOPA = 88:5:7, the solution concentration was 30%, magnetic stirring was used for dissolution, and nitrogen was introduced for deoxygenation for 40 minutes to obtain a first reaction system;

[0224] (3) adding azobisisobutylamidine hydrochloride (AIBA) with a mass concentration of 0.1% to the first reaction system, heating in a water bath at 50° C. for 6 hours to obtain a second reaction system;

[0225] (4) The second reaction system was repeatedly washed with anhydrous ethanol, and vacuum dried at 50° C. to obtain a mussel biomimetic temperature-resistant and salt-resistant thickener (p[AM-AANa-DOPA]), which was labeled as DS2.

[0226] In addition, the prepared mussel biomimetic temperature-resistant and salt-resistant thickener DS2 has the general formula shown in formula (4):

[0227]

[0228] Furthermore, in formula (4), m is 63, x is 6, and z is 10.

[0229] Comparative Example 3

[0230] The polymer DS1 (p[AM-AANa-AMPS]) in Comparative Example 1 was used as a thickener, and the preparation method of the supramolecular effect enhanced gel fracturing fluid was consistent with that of Example 3. The prepared supramolecular effect enhanced gel fracturing fluid was marked as D1.

[0231] like Figure 8 As shown, the viscosity recovery rate of the zirconium gel fracturing fluid prepared with tap water and 0.6% thickener (p[AM-AANa-AMPS]) after destructive shear is only 69.9%.

[0232] Comparative Example 4

[0233] The polymer DS2 (p[AM-AANa-DOPA]) in Comparative Example 2 was used as a thickener, and the preparation method of the supramolecular effect enhanced gel fracturing fluid was consistent with that of Example 3. The prepared supramolecular effect enhanced gel fracturing fluid was marked as D2.

[0234] Comparative Example 5

[0235] The polymer DS2 (p[AM-AANa-DOPA]) in Comparative Example 2 was used as a thickener, and the preparation method of the supramolecular effect enhanced gel fracturing fluid was consistent with that of Example 4. The prepared supramolecular effect enhanced gel fracturing fluid was marked as D3.

[0236] Test Case

[0237] The retained viscosity and shear recovery rate of the gel fracturing fluids prepared in Examples 4-8 and Comparative Examples 3-5 were tested as technical indicators. The results are shown in Table 2.

[0238] Among them, the shear rate is set to a constant 170s according to the performance evaluation method of water-based fracturing fluid in the petroleum and natural gas industry standard of the People's Republic of China (SY / T5107-2005). -1 , the temperature was raised to 200°C, the shear time was 2h, and the retained viscosity was obtained.

[0239] The shear recovery rate was obtained by a variable strain cyclic shear test, with the test temperature set at 25 °C and a constant angular frequency (ω = 6.28 rad·s -1 ), and perform strain sweep test with strain variation range of 1%-5000%. The two modulus curves will intersect and determine the critical failure point (intersection point of G' and G''). Then, take a value before and after the critical failure point to perform multiple cycles of shear strain oscillation sweep, which lasts for 600s under high shear failure strain and 100s under low shear strain. The elastic modulus recovery rate of the gel is calculated and the viscosity recovery ability of the gel is evaluated.

[0240] Table 1

[0241]

[0242] It can be seen from the results of Examples 4-8 and Comparative Examples 3-5 and Table 1 that the supramolecular action enhanced gel fracturing fluid prepared in Example 4 of the present invention exhibits good performance in terms of temperature resistance, shear resistance and self-repair. The supramolecular action enhanced zirconium gel fracturing fluid prepared with tap water and 0.6% thickener has a strength of 170s. -1 , sheared at 200℃ for 2h, the retained viscosity is as high as 85.7mPa·s, and the viscosity recovery rate after destructive shearing can reach 92.1%. The retained viscosity and shear recovery rate are very good, indicating that the supramolecular effect enhanced gel fracturing fluid has a high-strength non-covalent-covalent composite network structure. It has great application potential in the efficient fracturing of deep / ultra-deep oil and gas. In addition, the shear recovery rate of the DOPA-rich one is good, and the retained viscosity of the metal crosslinker is high.

[0243] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a gel fracturing fluid, characterized in that: The preparation method comprises: S201: contacting a mussel biomimetic heat-resistant and salt-resistant thickener with water to obtain a reaction system S201, wherein the mass ratio of the mussel biomimetic heat-resistant and salt-resistant thickener to water is (5-8): (992-995); wherein the mussel biomimetic heat-resistant and salt-resistant thickener has a structure shown in formula (1); Among them, m is 60-63, x is 4-7, y is 6-10, and z is 8-10; S202: Under stirring conditions, the reaction system S201 is contacted with a cross-linking agent to perform dissolution and aging reactions to obtain a gel fracturing fluid.

2. The preparation method according to claim 1, wherein The cross-linking agent is selected from one or more of organic zirconium, organic titanium, phenolic resin and polyethylene imine.

3. The preparation method according to claim 2, wherein The mass ratio of the organic zirconium to water is (5-16): (984-995).

4. The preparation method according to claim 2, wherein The mass ratio of the phenolic resin to water is (15-24):(976-985).

5. The preparation method according to claim 2, wherein: The mass ratio of the polyethyleneimine to water is (2-10):(990-998).

6. The preparation method according to any one of claims 1 to 5, wherein: When the cross-linking agent is organic zirconium, the reaction temperature is 65-80°C; Alternatively, when the cross-linking agent is a phenolic resin, the reaction temperature is 70-90°C; Alternatively, when the cross-linking agent is polyethyleneimine, the reaction temperature is 120-160°C.

7. The preparation method according to claim 1, wherein The preparation method of the mussel bionic temperature-resistant and salt-resistant thickener comprises: (1) in the presence of a xanthate-based water-soluble macromolecular chain transfer agent, contacting acrylamide, sodium acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 3-acrylamido dopamine and water to perform a reversible addition-fragmentation chain transfer polymerization reaction to obtain a first reaction system; (2) contacting the first reaction system with an initiator under water bath conditions to carry out heating reaction to obtain a second reaction system; (3) The second reaction system is cleaned and vacuum dried to obtain a mussel biomimetic temperature-resistant and salt-resistant thickener.

8. The preparation method according to claim 7, wherein: The molar ratio of acrylamide, sodium acrylate, 2-acrylamido-2-methylpropanesulfonic acid and 3-acrylamido dopamine is (63-75):(3-8):(5-15):(10-20); And / or, the initiator is azobisisobutyramidine hydrochloride; And / or, the mass ratio of the chain transfer agent to the initiator is (0.05-0.2): (0.3-0.5); and / or, in step (1), in the first reaction system, the concentration of the monomer solution is 30-40 wt %; And / or, in step (2), the conditions of the water bath include: temperature of 45-60° C. and time of 4-6 h.

9. The preparation method according to claim 7 or 8, wherein: The chain transfer agent has the general formula shown in formula (2): Among them, n is 5-10.

10. The preparation method according to claim 9, wherein: The preparation method of the chain transfer agent comprises: (e) contacting methyl 2-bromopropionate with methanol to dissolve the mixture and then cooling the mixture in an ice-water bath to obtain a reaction system e; (f) contacting the reaction system e with potassium ethyl xanthate to react to obtain a reaction system f; (g) removing the solvent from the reaction system f by vacuum rotary evaporation and then drying in a vacuum oven to obtain an intermediate product X; (h) contacting the intermediate product X, acrylamide, ethanol and water under nitrogen protection to obtain a reaction system h; (i) contacting the reaction system h with an initiator under water bath conditions to carry out heating reaction to obtain a reaction system i; (j) subjecting the reaction system i to vacuum rotary evaporation to remove the solvent and then subjecting the reaction system i to vacuum oven drying to obtain a chain transfer agent.

11. The preparation method according to claim 10, wherein: The molar ratio of methyl 2-bromopropionate and potassium ethyl xanthate is (4-6): (5-7); And / or, the molar ratio of the intermediate product X to acrylamide is (1-2):(5-10); And / or, the initiator is 4,4'-azobis(4-cyanovaleric acid); and / or, based on the total weight of methyl 2-bromopropionate and potassium ethyl xanthate, the amount of the initiator is 0.05-0.2 wt %; and / or, in step (e), the temperature of the ice water bath is -6°C to -2°C; And / or, in step (f), the reaction conditions include: temperature of 25-30°C, time of 12-20h; And / or, in step (i), the heating reaction temperature is 50-70°C and the time is 2-4h.

12. A gel fracturing fluid prepared by the preparation method according to any one of claims 1 to 11.

13. Use of the gel fracturing fluid according to claim 12 in fracturing development of deep / ultra-deep oil and gas reservoirs.