Conductive adhesive and its preparation method and application
By adding bismaleimide resin to the epoxy/anhydride curing system and combining silver powder, the problems of insufficient bonding strength of the conductive adhesive and serious chip warping are solved, and low warping and high temperature, humidity and heat conditions are achieved Interface bonding strength, suitable for semiconductor packaging and microelectronic devices.
Patent Information
- Application Number
- CN202311672275.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-07
AI Technical Summary
The existing conductive adhesives have problems such as insufficient interface bonding strength and serious chip warping in semiconductor packaging and microelectronic devices, especially in long-term high-temperature, low-temperature and humid-heat conditions, which leads to difficulty in using packaging materials.
Bismaleimide resin was added to the epoxy/anhydride curing system, combined with silver powder, and optimized the composition of the conductive adhesive to improve interface bonding strength and reduce chip warping.
Low chip warping under high temperature and humidity conditions is achieved, and the interface bonding strength of conductive adhesive is improved. The volume resistivity is 6.3×10-5 to 13×10-5Ω·cm, and the chip thrust and warpage are both Significant improvement.
Smart Images

Figure QLYQS_1 
Figure BDA0004593620900000021 
Figure BDA0004593620900000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a conductive adhesive and a preparation method and application thereof. Background Art
[0002] In the preparation and assembly of semiconductor packaging and microelectronic devices, adhesives play an important role. The basic functions include bonding, fixing, sealing protection, gap filling, grounding, insulation, etc. The main resin of the adhesive used for packaging is generally a thermosetting polymer material. In order to adapt to various subdivided applications, it is necessary to take into account the process performance of use and the functional properties after curing. For example, the process performance requires appropriate viscosity and rheological properties to meet high-speed dispensing, spraying or screen printing. The bonding performance directly reflects the firmness of the connection and fixation between the glue and various frame substrates, substrates, chips, etc. Considering the various possible working environments in which the chip is located, the bonding strength needs to be able to withstand the test of long-term high temperature, low temperature and humid heat conditions; the most common failure modes are: glue / frame delamination, cracking of the glue layer, chip warping, etc. A large number of studies have shown that the above phenomena are closely related to the thermal mismatch of the molding material, substrate, frame, glue and chip material itself. The difference in thermal expansion coefficient and modulus of different materials in contact with each other determine the degree of thermal mismatch. When the deformation caused by temperature change causes the internal stress accumulated inside the material to be unable to balance or exceed the interface bonding strength, the above failure may occur. As the chip package size increases, the chip warping, glue layer cracking, delamination, etc. caused by thermal mismatch are more serious, and the requirements for packaging materials are getting higher and higher.
[0003] Therefore, developing a conductive adhesive with low resistance, high bonding strength, good failure surface and low chip warping is an urgent problem to be solved in this field. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a conductive adhesive and a preparation method and application thereof, by adding a bismaleimide resin (BMI) into an epoxy / anhydride curing system, thereby effectively improving the interfacial bonding strength and achieving low chip warpage.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a conductive adhesive, the components of which include: a combination of bismaleimide resin, epoxy resin, anhydride curing agent and silver powder.
[0007] Preferably, the bismaleimide resin has a structure as shown in Formula 1;
[0008]
[0009] Wherein n is 5-20, for example, it can be 5, 6, 7, 8, 9, 10, 15, 18, 20, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the said range.
[0010] Preferably, the bismaleimide resin is a reddish brown viscous flowable liquid at 25°C.
[0011] Preferably, the viscosity of the bismaleimide resin at 25° C. and 10 rpm is 5-40 kcps, for example, 5 kcps, 6 kcps, 8 kcps, 10 kcps, 15 kcps, 20 kcps, 30 kcps, 35 kcps, 38 kcps, 40 kcps, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0012] As a preferred technical solution of the present invention, the bismaleimide resin having a structure as shown in Formula 1 is liquid at room temperature. Adding it to the epoxy / anhydride curing system effectively improves the interfacial bonding strength of the conductive adhesive and achieves low chip warpage.
[0013] BMI (bismaleimide) resin is an important electronic packaging material with excellent mechanical properties, high temperature resistance and moisture and heat resistance. However, due to the presence of a large number of cyclic rigid structures in its chemical structure, its melting point is very high. If it is dissolved with a solvent, a process step of solvent removal is required in subsequent use, so this type of material is inconvenient to process and use. In the present invention, a BMI resin that is a viscous liquid at room temperature is introduced into an epoxy resin / anhydride curing system.
[0014] Preferably, the bismaleimide resin is prepared by the following method, which comprises:
[0015] Maleimidopropionic acid, dicyclohexylcarbodiimide, polyether polyol, 4-dimethylaminopyridine and a solvent are mixed, reacted, filtered, extracted and dried to obtain the bismaleimide resin.
[0016] Preferably, the solvent comprises dichloromethane.
[0017] Preferably, the epoxy resin includes any one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenol novolac epoxy resin, methylphenol novolac epoxy resin, bisphenol A linear novolac epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, aralkyl epoxy resin, alicyclic epoxy resin, trifunctional epoxy resin or tetrafunctional epoxy resin, or a combination of at least two thereof.
[0018] Preferably, the anhydride curing agent includes any one of methyl nadic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, pyromellitic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, nadic anhydride, methyltetrahydrophthalic anhydride or methylhexahydrophthalic anhydride, or a combination of at least two thereof.
[0019] Preferably, the mass ratio of the anhydride curing agent to the epoxy resin is (0.8-0.9):1, for example, it can be 0.8:1, 0.82:1, 0.85:1, 0.88:1, 0.9:1, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0020] Preferably, the mass ratio of the bismaleimide resin to the epoxy resin is (0.2-0.4):1, for example, it can be 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0021] Preferably, the conductive adhesive further comprises: a curing accelerator, a silane coupling agent and a peroxide.
[0022] Preferably, the curing accelerator includes any one of 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole or 1-cyanoethyl-2-ethyl-4-methylimidazole, or a combination of at least two thereof.
[0023] The mass ratio of the curing accelerator to the epoxy resin is (0.5%-3%):1, preferably 1%:1.
[0024] Preferably, the silane coupling agent includes any one of γ-glycidyloxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane or N-aminoethyl-3-aminopropylmethyldimethoxysilane, or a combination of at least two thereof.
[0025] Preferably, the peroxide comprises cumene hydroperoxide, benzoyl peroxide BPO, tert-butyl peroxy-2-ethylhexanoate, di-tert-butyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxyneodecanoate, tert-amyl peroxy-2-ethylhexanoate (Arkema Luperox 575), cumene hydroperoxide (CHPO), di-tert-butyl peroxide (DTBP), diisopropyl peroxide (DCP), tert-amyl peroxyneodecanoate or diisopropyl peroxydicarbonate.
[0026] Preferably, the mass ratio of the silane coupling agent to the epoxy resin is 1:(50-100), for example, it can be 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0027] Preferably, the mass ratio of the peroxide to the bismaleimide resin is 1:(20-50), for example, it can be 1:20, 1:30, 1:40, 1:50, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0028] Preferably, the particle size of the silver powder is 0.3-30 μm, for example, it can be 0.3 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 29 μm, 30 μm, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0029] The amount of the silver powder is 3 to 4 times the mass of the components other than the silver powder, preferably 3 to 3.5 times. Too much silver powder may cause excessive adhesive viscosity and inconvenience in use; too little silver powder may cause excessive volume resistivity.
[0030] In a second aspect, the present invention provides an application of the conductive adhesive as described in the first aspect in the preparation or assembly of semiconductor packaging and microelectronic devices.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The conductive adhesive provided by the present invention adds bismaleimide resin to the epoxy / anhydride curing system, effectively improves the interface bonding strength, and achieves low chip warpage, with a volume resistivity of 6.3×10 -5 Up to 13×10 -5 Ω·cm, chip thrust is 7-12.5kgF at 23℃, 0.7-1.8kgF at 250℃, and chip warpage is <20μm. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] The experimental materials used in the embodiments and comparative examples of the present invention are as follows:
[0035] (1) Epoxy resin, 835LV, DIC Corporation;
[0036] (2) Anhydride curing agent, MeTHPA, Jiaxing Fulait Chemical Co., Ltd.;
[0037] (3) Silane coupling agent, KH560, KH570, Momentive;
[0038] (4) Curing accelerator, 2E4MZ, 2E4MZ-CN, Shikoku Chemical;
[0039] (5) Silver powder, EA-0295, Metalor Technologies USA;
[0040] (6) Polyether polyols, PPG-400, PPG-1000.
[0041] Preparation Example 1
[0042] This preparation example provides a bismaleimide resin, and the raw materials for preparing the bismaleimide resin include: maleimide propionic acid (253.5g, 1.5mol), dicyclohexylcarbodiimide (DCC) powder (309g, 1.5mol), PPG-400 (200g, 0.5mol), 4-dimethylaminopyridine (DMAP) powder (6.1g, 0.05mol) and 2800mL of dichloromethane.
[0043] The preparation method comprises:
[0044] Dissolve maleimide propionic acid in 2500mL of dichloromethane, then dissolve dicyclohexylcarbodiimide (DCC) powder in 300mL of dichloromethane. Under stirring, slowly drop dicyclohexylcarbodiimide DCC solution into maleimide propionic acid solution. After all the additions are completed, continue stirring and reacting for 10 minutes. Then add PPG-400 to the system; finally, slowly add 4-dimethylaminopyridine (DMAP) powder, and stop after 8 hours of reaction. Filter and filter out insoluble matter, take the filtrate and extract it with water in a separatory funnel, combine the organic layers, dry them over anhydrous Na2SO4, spin dry the filtrate to obtain a red viscous liquid, and a small amount of solid precipitates after standing and cooling. Filter again to obtain the final product BMI-PPG400. Yield: 98%.
[0045] The NMR data obtained from the test are as follows: 1 H NMR (600MHz, deuterated chloroform) δ6.66 (s, 4H), 3.76 (p, J = 7.9, 7.3Hz, 4H), 3.63–3.32 (m, 21H), 2.58 (t, J = 7.2Hz, 4H), 1.46–0.83 (m, 18H). The viscosity data measured at 10rpm was 25-30kcps. The viscosity test was based on the national standard GB / T22314-2008 "Method for Determination of Viscosity of Plastic Epoxy Resins", viscometer model: Anton Paar Rheolab QC, Z5 rotor.
[0046] Preparation Example 2
[0047] This preparation example provides a bismaleimide resin, and the raw materials for preparing the bismaleimide resin include: maleimide propionic acid (253.5 g, 1.5 mol), dicyclohexylcarbodiimide (DCC) powder (309 g, 1.5 mol), PPG-1000 (500 g, 0.5 mol), 4-dimethylaminopyridine (DMAP) powder (6.1 g, 0.05 mol) and 2800 mL of dichloromethane.
[0048] The preparation method comprises:
[0049] Dissolve maleimide propionic acid in 2500ml of dichloromethane, then dissolve dicyclohexylcarbodiimide (DCC) powder in 300ml of dichloromethane. Under stirring, slowly drop dicyclohexylcarbodiimide DCC solution into maleimide propionic acid solution. After all the additions are completed, continue stirring and reacting for 10 minutes. Then add PPG-1000 to the system; finally, slowly add 4-dimethylaminopyridine (DMAP) powder, and stop after 8 hours of reaction. Filter and filter out insoluble matter, take the filtrate and add water to extract in a separatory funnel, combine the organic layers, dry over anhydrous Na2SO4, spin dry the filtrate to obtain a red viscous liquid, and a small amount of solid precipitates after standing and cooling. Filter again to obtain the final product. Yield: 98%.
[0050] The NMR data obtained from the test are as follows: 1 H NMR (600 MHz, deuterated chloroform) δ 6.67 (s, 4H), 3.78 (t, J = 7.2 Hz, 4H), 3.61-3.26 (m, 52H), 2.60 (t, J = 7.1 Hz, 4H), 1.29-0.98 (m, 51H). The viscosity data measured at 10 rpm was 5-10 kcps.
[0051] Example 1
[0052] The present embodiment provides a conductive adhesive and a preparation method thereof. The components of the conductive adhesive include, by weight: 10 parts of epoxy resin 835L, 2 parts of bismaleimide resin BMI-PPG1000 (Preparation Example 2), 9 parts of anhydride curing agent MeTHPA, 0.1 parts of curing accelerator 2E4MZ-CN (Shikoku Chemical), 0.1 parts of isopropylbenzene hydroperoxide (CHPO), 0.2 parts of silane coupling agent KH-560 and 64.2 parts of silver powder.
[0053] The preparation method comprises:
[0054] Epoxy resin 835LV, BMI-PPG1000 (Preparation Example 2), acid anhydride MeTHPA, peroxide, cumene hydroperoxide (CHPO), and silane coupling agent KH-560 were weighed and added into a mixing kettle, mixed at 800 rpm for 15 min, then silver powder was added, dispersed at 800 rpm for 15 min, and then vacuum (vacuum degree <-0.095 MPa) degassed for 10 min, and discharged at normal pressure to obtain a conductive adhesive.
[0055] Embodiment 2-8
[0056] Example 2-8 provides a conductive adhesive and a preparation method thereof. The components of the conductive adhesive are shown in Table 1, and the preparation method is the same as that of Example 1.
[0057] Table 1
[0058]
[0059] x3 is three times the sum of the masses of the components except the silver powder.
[0060] Comparative Examples 1-4
[0061] Comparative Examples 1-4 provide a conductive adhesive and a preparation method thereof. The components of the conductive adhesive are shown in Table 2, and the preparation method is the same as that of Example 1.
[0062] Table 2
[0063]
[0064]
[0065] x3 is three times the sum of the masses of the components except the silver powder.
[0066] The performance of the conductive adhesives provided in Examples 1-8 and Comparative Examples 1-4 was tested in the following manner:
[0067] (1) Adhesive strength: The test method refers to "HG / T 5912-2021 Conductive Adhesives", the silicon wafer size is: 2mmx2mm; the substrate is a silver-plated copper sheet, the curing conditions are an oven at 175℃x1h; the test equipment is a DAGE-4000P multi-function push-pull test machine, Nordson DAGE Precision Industries LTD, USA, and the shear strength is the thrust size (unit is kgF); 5 samples of each adhesive are taken and the average value is taken;
[0068] (2) Residual adhesive rate (evaluation of the damaged surface): Observe the residual adhesive on the substrate after the thrust damage through an optical microscope, and evaluate the area ratio of the residual adhesive part (percentage relative to the chip area). Take the arithmetic average of 10 samples;
[0069] (3) Warpage measurement: A silver-plated frame is used, the chip size is 9mmx9mm, and it is baked and cured at 175℃x1h. The chip surface warpage is measured by microscope, and the unit is um. If the warpage exceeds 20um, it is considered unqualified (test equipment: Keyence microscope VHX-7100);
[0070] (4) The volume resistivity test is carried out in accordance with the four-probe method of the industry standard "HG / T 5912 Conductive Adhesives";
[0071] Preparation of conductive film: On a glass substrate, a conductive adhesive with a thickness of 25um, a width of 9mm, and a length of 50mm was prepared by a controlled thickness tape scraping method. It was baked and cured in an oven at 175°C for 60min; resistance tester: Changzhou Tonghui Electronics Co., Ltd., TH2516 DC resistance tester.
[0072] The performance of the conductive adhesives provided in Examples 1-8 and Comparative Examples 1-4 was tested, and the test results are shown in Tables 3-4.
[0073] Table 3
[0074]
[0075] Table 4
[0076]
[0077]
[0078] By comparing the performance of each embodiment, it can be found that: in terms of volume resistivity, there is little change compared to not adding bismaleimide resin (Comparative Example 1). When the amount of anhydride curing agent is slightly less, the volume resistivity increases slightly. When the bismaleimide resin (Preparation Example 2) replaces the bismaleimide liquid resin (Preparation Example 1), the volume resistivity is slightly larger under the same conditions (Example 7 relative to Example 2; Example 8 relative to Example 5).
[0079] In terms of thrust, when bismaleimide resin is not included, the normal temperature thrust is large, but the high temperature thrust is small, and the residual surface is zero; when the bismaleimide resin content increases (such as Examples 1 / 2 / 3), the thrust decreases slightly, but the high temperature thrust is good, and the residual surface is above 40%; when bismaleimide resin (Preparation Example 2) replaces bismaleimide resin (Preparation Example 1), the normal temperature / high temperature thrust decreases under the same conditions; but the damage surface is better; the bismaleimide resin content in Comparative Example 2 is too high, and the corresponding normal temperature and high temperature thrust of the chip are low, but the volume resistivity is too large. Comparative Examples 3 and Comparative Examples 4 correspond to the cases of insufficient anhydride and excessive anhydride, respectively. Compared with Example 2, the normal temperature thrust of the two is lower, the high temperature thrust is lower, but the chip warping is better; the volume resistivity of Comparative Example 3 is larger, increasing by 2 orders of magnitude to 10 -3 Ω·cm.
[0080] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a conductive adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A conductive adhesive, characterized in that: The conductive adhesive is composed of the following components: a combination of bismaleimide resin, epoxy resin, anhydride curing agent, silver powder, curing accelerator, silane coupling agent and peroxide; the mass ratio of the bismaleimide resin to the epoxy resin is (0.2-0.4):1; the mass ratio of the anhydride curing agent to the epoxy resin is (0.8-0.9):1; the epoxy resin is epoxy resin 835LV; The bismaleimide resin has a structure as shown in Formula 1; ; Formula 1 Where n is 5-20.
2. The conductive adhesive according to claim 1, characterized in that: The bismaleimide resin is a reddish brown mobile liquid at 25°C.
3. The conductive adhesive according to claim 1, characterized in that: The bismaleimide resin has a viscosity of 5-40 kcps at 25° C. and 10 rpm.
4. The conductive adhesive according to claim 1, characterized in that: The acid anhydride curing agent includes any one of methyl nadic anhydride, methyl tetrahydrophthalic anhydride, methyl hexahydrophthalic anhydride, pyromellitic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, and nadic anhydride, or a combination of at least two thereof.
5. Use of the conductive adhesive according to any one of claims 1 to 4 in semiconductor packaging, preparation or assembly of microelectronic devices.