Composition for preparing anti-slip film and backing paper for transporting display panels manufactured using the same

By using the anti-slip film prepared by a specific composition on the liner for display panel transportation, the problems of flow and scratches in the transportation of light and thin display panels are solved, and stable transportation and anti-static properties are achieved in high temperature and high humidity environments, satisfying the The protection requirements of modern display panels.

CN117683316BActive Publication Date: 2024-11-15KOREA KUMHO PETROCHEMICAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311159702.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2023-09-08
Publication Date
2024-11-15
Estimated Expiration
2043-09-08

AI Technical Summary

Technical Problem

The existing liner paper for transportation for display panels is damaged and scratched by the protective film due to flow during transportation, and the adhesion is reduced in high temperature and high humidity environment, making it difficult to meet the protection needs of lightweight and high-resolution display panels. .

Method used

A composition comprising 60-90 parts by weight of a viscosity enhancer, 20-80 parts by weight of an olefin-based elastomer, 15-30 parts by weight of an olefin-based resin and 20-30 parts by weight of a conductive component for preparation Anti-slip film is formed on the foam sheet to ensure anti-static and heat resistance.

Benefits of technology

It realizes stable transportation of the display panel in high temperature and high humidity environments, reduces flow and scratches, maintains excellent anti-slip and anti-static properties, and prevents the liner from sticking to the panel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117683316B_ABST
    Figure CN117683316B_ABST
Patent Text Reader

Abstract

One embodiment of the present specification provides a composition for preparing an anti-skid film and a backing paper for transporting a display panel manufactured using the same. The composition for preparing the anti-skid film comprises, relative to 100 parts by weight of a thermoplastic elastomer other than an olefin elastomer: 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an olefin elastomer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composition for preparing an anti-slip film and a lining paper for transporting a display panel manufactured by using the composition. Background Art

[0002] The display panel has a shape that is extremely vulnerable to external impacts, so in order to protect the panel, packaging materials are used for transportation to deal with the risk of damage to the panel during transportation. The packaging material used between panels in the packaging for this purpose is called lining paper. The early panels used in the past had thicker glass used in the panels, so there was almost no panel damage caused by panel flow generated during product transportation. However, as the design of display products such as TVs, monitors, and tablets has gradually tended to be lighter and higher resolution, the thickness of the glass used in the panels has gradually become thinner. Therefore, in recent years, panel damage caused by flow generated during transportation has increased rapidly. In addition, according to the current trend of not removing the panel POL protective film during the process in order to simplify the process, scratches on the protective film frequently occur due to the friction between the lining paper and the panel caused by the panel flow that occurs during transportation.

[0003] The friction coefficient between the existing display transport backing paper and the panel is low, so it flows severely during transportation, resulting in frequent damage to the panel. In addition, even if the friction coefficient of the backing paper is increased, the protective film is easily scratched due to the high hardness of the backing paper surface. Therefore, it is necessary to develop a new backing paper that can minimize the flow of the panel during transportation and reduce the occurrence of scratches.

[0004] In addition, existing anti-slip lining papers utilize self-adhesiveness to increase the coefficient of friction to prevent the panels from flowing during transportation, but various side effects occur, such as adhesion and transfer to the panels and decreased adhesion over time, and therefore are not used in practice. When passing through the equatorial region, where the transportation environment is poor due to high humidity and temperature, the problem of related flow phenomena becomes more serious. Summary of the invention

[0005] The present invention is developed to solve the problems disclosed in the above-mentioned prior art. One of the multiple objects of the present invention is to provide a composition for preparing an anti-slip film having excellent heat resistance.

[0006] Another object of the present invention is to provide a liner for transporting display panels that has excellent anti-slip properties, exhibits sustained antistatic properties, and does not adhere to the surface.

[0007] According to one aspect, a composition for preparing an anti-skid film is provided. The composition for preparing an anti-skid film includes, relative to 100 parts by weight of a thermoplastic elastomer (excluding olefin elastomer): 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an olefin elastomer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component.

[0008] In one embodiment, the thermoplastic elastomer may be a styrene-butadiene-styrene (SBS) block copolymer having a styrene content of 28 wt % to 35 wt % and a weight average molecular weight of 40,000 g / mol to 200,000 g / mol.

[0009] In one embodiment, the diblock content of the styrene-butadiene-styrene block copolymer may be less than 40 wt %.

[0010] In one embodiment, the above-mentioned styrene-butadiene-styrene block copolymer may include a first styrene-butadiene-styrene block copolymer having a diblock content of less than 40 weight % and a second styrene-butadiene-styrene block copolymer having a diblock content greater than 40 weight %, and a weight ratio of the above-mentioned first styrene-butadiene-styrene block copolymer to the above-mentioned second styrene-butadiene-styrene block copolymer may be greater than 7:3 and less than 10:0.

[0011] In one embodiment, the tackifier may be one selected from the group consisting of aromatic oil, cyclohexane oil, paraffin oil and combinations thereof.

[0012] In one embodiment, the olefin resin may be polypropylene resin.

[0013] In one embodiment, the olefin resin may have a melting temperature of 130° C. or higher and a melt flow index of 0.1 g / 10 min to 12 g / 10 min.

[0014] In one embodiment, the olefin-based elastomer may have a melting temperature of less than 65° C. and a melt flow index of 0.1 g / 10 min to 20 g / 10 min.

[0015] In one embodiment, the conductive component may be one selected from the group consisting of conductive carbon black, carbon nanotubes, and combinations thereof.

[0016] In one embodiment, the conductive carbon black may be one selected from the group consisting of Ketjen black, acetylene black, furnace black, channel black, ultra-high carbon black and combinations thereof.

[0017] In one embodiment, the carbon nanotubes may be bundled carbon nanotubes, with an average bundle diameter of 0.5 μm to 20 μm, an average bundle length of 10 μm to 200 μm, and an apparent density of 0.005 g / mL to 0.120 g / mL.

[0018] In one embodiment, the conductive component may include conductive carbon black and carbon nanotubes in a weight ratio of 1:1 to 3:1.

[0019] In one embodiment, the composition for preparing the anti-slip film may further include polyoctenes.

[0020] In one embodiment, the content of the polyoctenylene may be 5 parts by weight to 20 parts by weight, and the ratio of double bond CIS may be 10% to 30%.

[0021] In one embodiment, the polyoctene may have a melting temperature of 50°C to 70°C.

[0022] According to another aspect, a lining paper for transporting a display panel is provided, comprising: a foam sheet; and an anti-slip film formed on at least one side of the foam sheet, wherein the anti-slip film comprises a cured product of the composition for preparing the anti-slip film.

[0023] In one embodiment, the foam sheet may be one selected from the group consisting of polyethylene, polypropylene, ethylene vinyl acetate (EVA), polyurethane, and combinations thereof.

[0024] The interlining paper for transporting a display panel prepared using the composition for preparing an anti-slip film according to one aspect of the present invention has excellent anti-slip performance, antistatic performance and outstanding film-forming property.

[0025] Furthermore, the interleaving paper for transporting a display panel according to another aspect of the present invention exhibits antistatic properties by ensuring dispersibility of a conductive component, and by ensuring heat resistance, the interleaving paper does not adhere to a display even if the panel is transported in a high temperature and high humidity environment.

[0026] The effects of one aspect of the present invention are not limited to the above-mentioned effects, and should be understood to include all effects inferred from the structure of the invention described in the detailed description of this specification or the claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 FIG. 1 is a conceptual diagram showing an example of a liner for shipping a display panel according to the present invention.

[0028] Figure 2 FIG. 1 is a conceptual diagram showing another example of a slip sheet for shipping a display panel according to the present invention.

[0029] Description of Reference Numerals

[0030] 10: Anti-slip film

[0031] 20: Foam sheet

[0032] 100: Backing paper for transporting single-sided laminated display panels

[0033] 200: Double-sided laminated display panel transportation backing paper DETAILED DESCRIPTION

[0034] Hereinafter, one aspect of the present specification will be described with reference to the accompanying drawings. However, the contents of the present specification can be implemented in many different forms and are not limited to the embodiments described in the present specification.

[0035] Throughout the specification, when it is described that a component is “connected” to another component, it includes not only the case of “direct connection” but also the case of “connected with other components interposed therebetween.” Furthermore, when a component is referred to as “including (or comprising)” an element, unless expressly specified otherwise, instead of excluding any other elements, it may mean that a component may further include other elements.

[0036] In this specification, when describing a series of numerical ranges, unless otherwise specifically stated, these values ​​have a precision of significant figures provided according to standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.

[0037] Composition for preparing anti-slip film

[0038] According to one aspect of the present specification, the composition for preparing an anti-slip film includes, relative to 100 parts by weight of a thermoplastic elastomer (excluding olefin elastomer), 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an olefin elastomer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component.

[0039] The thermoplastic elastomer (TPE) is a component added to impart viscoelasticity to the anti-slip film, and may be one selected from the group consisting of styrene-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, fluorine-based thermoplastic elastomers, polyester-based thermoplastic elastomers, PVC-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, and combinations of two or more thereof. For example, the thermoplastic elastomer may be a styrene-based thermoplastic elastomer, but is not limited thereto, and a thermoplastic elastomer having viscoelasticity may be used without limitation.

[0040] The above-mentioned styrene-based thermoplastic elastomer can be one of the group consisting of styrene-butadiene-styrene (SBS) copolymer, styrene-isoprene-styrene (SIS) copolymer, styrene-ethylene-propylene-styrene (SEPS) copolymer, styrene-butadiene-butylene-styrene (SBBS) copolymer, styrene-ethylene-butylene-styrene (SEBS) copolymer and a combination of two or more thereof, for example, it can be a styrene-butadiene-styrene block copolymer, but is not limited thereto.

[0041] The styrene-based thermoplastic elastomer may be a styrene-butadiene-styrene block copolymer having a styrene content of 28 to 35 wt % and a weight average molecular weight of 40,000 to 200,000 g / mol.

[0042] Styrene content refers to the weight proportion of styrene in the total weight of the corresponding block copolymer, which can usually be measured by nuclear magnetic resonance spectroscopy (NMR). If the styrene content of the above-mentioned styrene-butadiene-styrene block copolymer is less than 28% by weight, the elasticity may increase and the anti-slip performance may deteriorate. If the styrene content of the above-mentioned styrene-butadiene-styrene block copolymer is greater than 35% by weight, the viscosity increases and panel contamination and adhesion may occur.

[0043] If the weight average molecular weight of the above-mentioned styrene-butadiene-styrene block copolymer is less than 40,000 g / mol, the viscosity of the material increases, the heat resistance decreases, and the possibility of the panel being contaminated during use may increase. If the weight average molecular weight of the above-mentioned styrene-butadiene-styrene block copolymer is above 200,000 g / mol, the elasticity increases, which may have an adverse effect on the anti-slip performance.

[0044] The diblock content of the styrene-butadiene-styrene block copolymer may be 40 wt% or less. If the diblock content of the styrene-butadiene-styrene block copolymer exceeds 40 wt%, the viscosity is too high, the heat resistance is reduced, and panel contamination may occur.

[0045] The styrene-butadiene-styrene block copolymer may include a first styrene-butadiene-styrene block copolymer having a diblock content of 40% by weight or less and a second styrene-butadiene-styrene block copolymer having a diblock content of more than 40% by weight, in which case the proportion of the second styrene-butadiene-styrene block copolymer relative to the entire styrene-butadiene-styrene block copolymer may be 30% by weight or less. If the content of the second styrene-butadiene-styrene block copolymer exceeds 30% by weight, the viscosity is too high, the heat resistance is reduced, and panel contamination may occur.

[0046] The tackifier is a component added to increase the viscosity of the thermoplastic elastomer, and may be one selected from the group consisting of aromatic oil, naphthenic oil, paraffin oil, and a combination thereof, but is not limited thereto.

[0047] Relative to 100 parts by weight of the above-mentioned thermoplastic elastomer, the content of the above-mentioned tackifier can be 60 parts by weight to 90 parts by weight, for example, it can be 60 parts by weight, 61 parts by weight, 62 parts by weight, 63 parts by weight, 64 parts by weight, 65 parts by weight, 66 parts by weight, 67 parts by weight, 68 parts by weight, 69 parts by weight, 70 parts by weight, 71 parts by weight, 72 parts by weight, 73 parts by weight, 74 parts by weight, 75 parts by weight, 76 parts by weight, 77 parts by weight, 78 parts by weight, 79 parts by weight, 80 parts by weight, 81 parts by weight, 82 parts by weight, 83 parts by weight, 84 parts by weight, 85 parts by weight, 86 parts by weight, 87 parts by weight, 88 parts by weight, 89 parts by weight, 90 parts by weight or a range between two of the values. If the content of the thickener is less than the above range, the elasticity may increase and the anti-slip performance may deteriorate. If the content of the thickener exceeds the above range, the viscosity may increase excessively, causing the display panel to be contaminated by the backing paper, or dissolution may occur on the panel surface.

[0048] The olefin-based elastomer is a component added to promote film formation and enhance adhesion, and may be one selected from the group consisting of ethylene-based elastomers, propylene-based elastomers, and combinations thereof, but is not limited thereto.

[0049] The ethylene-based elastomer or the propylene-based elastomer may include a combination of ethylene and propylene, and may be a copolymer further including an additional polymerizable monomer in addition to ethylene or propylene.

[0050] For example, the ethylene-based elastomer may be an ethylene / α-olefin block copolymer, wherein ethylene accounts for at least 50 mol% of the entire polymer and the substantial remainder includes α-olefins having three or more carbon atoms as monomers. In this case, the α-olefin may be propylene, 1-butene, 1-hexene or 1-octene.

[0051] For example, the propylene-based elastomer may be a block copolymer in which propylene accounts for at least 50 mol% of the entire polymer and the remaining portion includes ethylene or an α-olefin having four or more carbon atoms as a monomer. In this case, the α-olefin may be 1-hexene or 1-octene.

[0052] The melting temperature of the olefin elastomer may be less than 65° C. If the melting temperature of the olefin elastomer exceeds 65° C., the hardness of the film increases, which may adversely affect the anti-slip property.

[0053] The melt flow index of the olefin elastomer may be 0.1 g / 10 min to 20 g / 10 min, preferably 0.1 g / 10 min to 10 g / 10 min, in which case a thinner film may be easily formed, but the present invention is not limited thereto.

[0054] The content of the olefin elastomer may be 20 to 80 parts by weight relative to 100 parts by weight of the thermoplastic elastomer, for example, the content of the olefin elastomer may be 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, or a range between two values. If the content of the olefin elastomer is less than the above range, it is difficult to form a film, and if the content of the olefin elastomer exceeds the above range, heat resistance may be adversely affected.

[0055] The above-mentioned olefin resin is a component added to ensure that the anti-slip film does not adhere to the display panel under high temperature and high humidity transportation environment and maintains strength even after the film is formed. As long as its melting temperature is above 130°C, its type is not limited. For example, it can be at least one selected from the group consisting of HDPE (high-density polyethylene) resin, LDPE (low-density polyethylene) resin, LLDPE (linear low-density polyethylene) resin, polypropylene resin and ethylene-propylene copolymer resin. Preferably, it can be polypropylene resin.

[0056] The melt flow index of the olefin resin may be 0.1 g / 10 min to 12 g / 10 min, preferably 0.1 g / 10 min to 2 g / 10 min, in which case a thinner film may be easily formed, but the present invention is not limited thereto.

[0057] The content of the olefin resin may be 15 to 30 parts by weight relative to 100 parts by weight of the thermoplastic elastomer. For example, the content of the olefin resin may be 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, or any range therebetween. If the content of the olefin resin is lower than the above range, the surface of the display panel and the backing paper may adhere to each other under high temperature and high humidity conditions, and the surface may be damaged. If the content of the olefin resin exceeds the above range, the anti-slip property may be adversely affected.

[0058] The conductive component is added to prevent static electricity, ensure heat resistance and reduce surface resistance, and may be one selected from the group consisting of conductive carbon black, carbon nanotubes and a combination thereof, but is not limited thereto.

[0059] The carbon black may be one selected from the group consisting of ketjen black, acetylene black, furnace black, channel black, timcal carbon black, and mixtures thereof, and ketjen black having excellent conductivity may be used, but is not limited thereto.

[0060] The carbon nanotubes may be bundled carbon nanotubes, but are not limited thereto.

[0061] The carbon nanotubes may have an average bundle diameter of 0.5 μm to 20 μm, an average bundle length of 10 μm to 200 μm, and an apparent density of 0.005 g / mL to 0.120 g / mL, but are not limited thereto.

[0062] The conductive component may include conductive carbon black and carbon nanotubes in a weight ratio of 1:1 to 3:1. For example, the weight ratio of conductive carbon black to carbon nanotubes may be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, or a value between any two of the above weight ratios. The higher the ratio of carbon black, the more advantageous in terms of anti-slip properties, and the higher the ratio of carbon nanotubes, the more advantageous in terms of resistance value, but are not limited to the above ranges.

[0063] Relative to 100 parts by weight of the above-mentioned thermoplastic elastomer, the content of the above-mentioned conductive component can be 20 parts by weight to 30 parts by weight. For example, the content of the above-mentioned conductive component can be 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight or a range between two values.

[0064] The composition for preparing the anti-slip film may further include polyoctenamer to enhance the anti-slip performance.

[0065] The melting temperature of the polyoctenes may be 50° C. to 70° C., and may have a CIS and TRANS structure with a CIS ratio of double bonds of 10% to 30%, but is not limited thereto. The anti-slip property may be enhanced by adding polyoctenes. If the ratio of CIS in the double bonds of the polyoctenes is less than 10%, the viscosity may be too strong and adhesion may occur on the surface of the display panel, and if the ratio of CIS in the double bonds of the polyoctenes is more than 30%, the elasticity may be too strong, and thus the anti-slip property may be offset.

[0066] The content of the polyoctenylene may be 5 to 20 parts by weight relative to 100 parts by weight of the thermoplastic elastomer, for example, the content of the polyoctenylene may be 5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight, or a value between these two values. If the content of the polyoctenylene is less than the above range, the effect of enhancing the anti-slip performance is not great, and if the content of the polyoctenylene exceeds the above range, the viscosity of the adhesion enhancer may be weakened, thereby reducing the anti-slip effect.

[0067] The composition for preparing the anti-slip film may further include pigments or other additives to achieve color.

[0068] Display panel shipping backing paper

[0069] According to another aspect of the present invention, a display panel transport backing paper comprises: a foam sheet; and an anti-skid film formed on at least one side of the foam sheet, wherein the anti-skid film comprises a solidified product of the composition for preparing the anti-skid film. Furthermore, the foam sheet is one selected from the group consisting of polyethylene, polypropylene, ethylene vinyl acetate, polyurethane, and a combination thereof.

[0070] Figure 1 A cross-sectional view showing a single-sidedly-bonded display panel shipping backing paper 100 as one example of the display panel shipping backing paper, ie, in which the foam sheet 10 is attached to only one side of the anti-slip film 20 .

[0071] Figure 2 As one example of the display panel shipping backing paper, a cross-sectional view showing a double-sided laminating type display panel shipping backing paper 200 in which the foam sheet 10 is attached to both surfaces of the anti-slip film 20 is shown.

[0072] The above-mentioned display panel transportation backing paper exhibits excellent anti-slip performance and excellent antistatic performance and has low hardness, so it can be used to transfer parts during the transportation and manufacturing process of electronic and electrical products, but is not limited to this and can be applied to various fields requiring anti-slip performance.

[0073] The above-mentioned display panel transport backing paper has excellent anti-slip properties, so it can prevent the display panel from sliding when transporting it in a high temperature and high humidity environment. Therefore, no matter what the size, position and shape of the display panel is, the panel can be stably transported by using a flat anti-slip backing paper.

[0074] The above-mentioned backing paper for transporting display panels can be manufactured by a film extrusion process, a laminating process and a cutting process. In the above-mentioned film extrusion process, a non-slip film with a thickness of 10 μm to 100 μm is prepared by extruding a non-slip material, in the above-mentioned laminating process, the non-slip film and a foam sheet with a thickness of 0.5 mm or more are hot-melted and laminated, and in the above-mentioned cutting process, the manufactured backing paper is cut according to size by a press, but the manufacturing process of the backing paper for transporting display panels is not limited thereto.

[0075] The above-mentioned interleaving paper for transporting display panels can be manufactured into various thicknesses according to the application, for example, can be manufactured into a thickness of 0.5 mm to 2 mm, but is not limited thereto.

[0076] The above-mentioned display panel shipping interleaving paper can be manufactured in various colors by adding dyes during the manufacturing process.

[0077] The display panel transport backing paper may be formed by laminating the anti-slip film and the foam sheet. The thickness of the foam sheet may be greater than 0.5 mm, but is not limited thereto.

[0078] The surface resistance of the above-mentioned anti-slip backing paper measured according to ASTM D257 can be 10 6 Ω / sq to 10 10 Ω / sq.

[0079] Hereinafter, embodiments of the present invention will be described in more detail. However, the following experimental results are only representative experimental results in the above-mentioned embodiments, and the embodiments etc. should not be construed as limiting or restricting the scope and content of this specification. The effects of various embodiments of this specification that are not clearly presented below are specifically recorded in the corresponding parts.

[0080] Example

[0081] Use twin screw extruder ( L / D 36) A composition comprising a styrene-butadiene-styrene block copolymer, a tackifier, an olefin elastomer, an olefin resin, a conductive component, polyoctene and other additives was extruded at 180° C. to 210° C. at a screw speed of 200 rpm to prepare the anti-slip films of Examples 1 to 6 of the present invention and Comparative Examples 1 to 6.

[0082] Here, the thermoplastic elastomer, tackifier, olefin elastomer, olefin resin, conductive component, and polyoctenes used in Inventive Examples 1 to 6 and Comparative Examples 1 to 6 are as follows.

[0083] -Styrene-butadiene-styrene block copolymer 1 (SBS1): a styrene-butadiene-styrene block copolymer having a styrene content of 32 parts by weight, a weight average molecular weight of 120,000 g / mol, and a diblock content of 35%

[0084] -Styrene-butadiene-styrene block copolymer 2 (SBS2): a styrene content of 32 parts by weight, a weight average molecular weight of 120,000 g / mol, and a diblock content of 65%

[0085] -Thickener: Kinematic viscosity at 40°C is 50 mm 2 / s and a paraffin oil with a pouring point of -15°C

[0086] -Olefin elastomer: Engage 8150 (ethylene-octene polyolefin elastomer) from Dow

[0087] -Olefin resin: polypropylene resin with MI = 2g / 10min

[0088] -Conductive carbon black: Ketjen Black EC600JD from Akzo Nobel

[0089] -Carbon nanotubes: Kumho Petrochemical's K-Nanos 210T

[0090] -Polyoctene: Polyoctene with a melting point of 55°C and a double bond CIS / TRANS ratio of 2 / 8

[0091] The contents of the components of the compositions used to prepare the anti-slip films of Inventive Examples 1 to 6 and Comparative Examples 1 to 6 are shown in Tables 1 and 2 below.

[0092] Table 1

[0093]

[0094]

[0095] Table 2

[0096]

[0097] Experimental example

[0098] Experimental Example 1: Surface resistance measurement

[0099] According to ASTM D257, the surface resistance of a flat plate sample having a thickness of 2 mm was measured 5 times using an ohmmeter (Ohmmeter, USA, Static Solutions, Inc., OHM-STAT RT-1000) as a surface resistance measuring device in an environment of 24° C. temperature and 47% humidity, and the average value was calculated.

[0100] Experimental Example 2: Anti-slip Performance Evaluation 1) Friction Coefficient Measurement

[0101] The material for preparing the anti-slip film was pressed in a 150° C. hot press to make a film having a thickness of 100 μm, and then the friction coefficient was measured according to ASTM D 1894. At this time, stainless steel (SUS) was used as a friction body.

[0102] Experimental Example 3: Anti-slip Performance Evaluation 2) Sliding Angle Measurement

[0103] After the above-mentioned display panel transporting backing paper is manufactured and fixed, the display panel is placed thereon, and then the angle at which the display panel starts to slide is measured.

[0104] Experimental Example 4: Reliability Evaluation 1) High Temperature and High Humidity Test

[0105] After placing the backing paper on a 50-inch display panel, test it in an environment of 60°C temperature and 90% humidity for 240 hours, and then place it at room temperature for 24 hours. If the backing paper and the panel are not adhered and the components of the backing paper are not transferred to the panel, it is judged as "qualified", and if the backing paper and the panel are adhered or the components of the backing paper are transferred to the panel, it is judged as "unqualified".

[0106] Experimental Example 5: Reliability Evaluation 2) Vibration Test

[0107] The scratches and damage on the panel surface were evaluated by placing a backing paper on a 50-inch display panel and then vibrating it for 24 hours. If there were no scratches or damage, it was judged as "pass", otherwise it was judged as "fail".

[0108] Experimental Example 6: Film Formation Evaluation

[0109] The display panel transport backing paper is made into a thickness of about 1 mm and heated to 180 degrees, and then stretched at a speed of 500 m / min. If it is stretched by more than 100%, it is judged as "qualified", otherwise it is judged as "unqualified".

[0110] The evaluation results of the surface resistance, friction coefficient, sliding angle, high temperature and high humidity, vibration and film forming properties of Experimental Examples 1 to 6 are shown in Tables 3 and 4 below.

[0111] Table 3

[0112]

[0113] Referring to Table 3, the samples prepared using the compositions of Inventive Examples 1 to 6 have a friction coefficient of 3.5 or more and a sliding angle of 60° or more, showing excellent anti-slip performance. In addition, there is no performance degradation under high temperature and high humidity conditions, no panel damage caused by vibration, and excellent film forming properties.

[0114] Table 4

[0115]

[0116]

[0117] Referring to Table 4 above, the samples of Comparative Examples 1 and 6 using styrene-butadiene-styrene block copolymer (SBS2) with a diblock content of more than 30 wt% and greater than 40 wt% show excellent surface resistance and anti-slip properties, but the performance of the backing paper deteriorates under high temperature and high humidity, and the film-forming properties do not meet the qualified standards.

[0118] The film-forming property of the sample of Comparative Example 2 in which the olefin elastomer content is less than 20 parts by weight is deteriorated, and the anti-slip performance and backing paper performance of the sample of Comparative Example 3 in which the olefin elastomer content is greater than 80 parts by weight are reduced compared with Example 1 of the present invention, for example, damage to the panel is caused under high temperature, high humidity and vibration conditions.

[0119] Compared with Inventive Example 1, the sample prepared from the composition of Comparative Example 4 having an olefin resin content exceeding 30 parts by weight had reduced anti-slip properties such as friction coefficient and sliding angle, and did not pass the test based on vibration. In addition, the sample prepared from the composition of Comparative Example 5 having an olefin resin content of less than 15 parts by weight had a friction coefficient and sliding angle similar to those of Inventive Example 1, but affected the panel under high temperature and high humidity, and the film-forming property deteriorated.

[0120] The above description of this specification is only illustrative, and anyone skilled in the art of the present specification will understand that it can be easily transformed into other specific forms without changing the technical ideas or essential features of the present specification. Therefore, it should be understood that the above-mentioned embodiments are only illustrative in all aspects, but are not limited to this. For example, each structural component described as a single type can also be implemented in a dispersed manner, and similarly, the structural components described in a dispersed manner can also be implemented in a combined form.

[0121] The scope of the present specification is indicated by the appended claims rather than the above detailed description, and all changes or modifications derived from the meaning, scope and equivalent concepts of the claims should be interpreted as being included in the scope of the present specification.

Claims

1. A composition for preparing an anti-slip film, characterized in that: Relative to 100 parts by weight of the thermoplastic elastomer other than the olefin elastomer, including: 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an ethylene / α-olefin block copolymer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component, The olefin resin is at least one selected from the group consisting of high-density polyethylene resin, low-density polyethylene resin, linear low-density polyethylene resin, polypropylene resin and ethylene-propylene copolymer resin. The thermoplastic elastomer is a styrene-butadiene-styrene block copolymer having a styrene content of 28 wt % to 35 wt % and a weight average molecular weight of 40000 g / mol to 200000 g / mol. The diblock content of the styrene-butadiene-styrene block copolymer is 40% by weight or less.

2. A composition for preparing an anti-skid film, characterized in that: Relative to 100 parts by weight of the thermoplastic elastomer other than the olefin elastomer, including: 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an ethylene / α-olefin block copolymer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component, The olefin resin is at least one selected from the group consisting of high-density polyethylene resin, low-density polyethylene resin, linear low-density polyethylene resin, polypropylene resin and ethylene-propylene copolymer resin. The thermoplastic elastomer is a styrene-butadiene-styrene block copolymer having a styrene content of 28 wt % to 35 wt % and a weight average molecular weight of 40000 g / mol to 200000 g / mol. The styrene-butadiene-styrene block copolymer comprises a first styrene-butadiene-styrene block copolymer having a diblock content of 40 wt % or less and a second styrene-butadiene-styrene block copolymer having a diblock content of more than 40 wt %. A weight ratio of the first styrene-butadiene-styrene block copolymer to the second styrene-butadiene-styrene block copolymer is 7:3 or more and less than 10:

0.

3. The composition for preparing an anti-slip film according to claim 1 or 2, characterized in that: The above-mentioned tackifier is one selected from the group consisting of aromatic oil, naphthenic oil, paraffin oil and a combination thereof.

4. The composition for preparing an anti-slip film according to claim 1 or 2, characterized in that: The above-mentioned olefin resin is polypropylene resin.

5. The composition for preparing an anti-slip film according to claim 1 or 2, characterized in that: The conductive component is one selected from the group consisting of conductive carbon black, carbon nanotubes and a combination thereof.

6. The composition for preparing an anti-slip film according to claim 5, characterized in that: The conductive carbon black includes one selected from the group consisting of Ketjen black, acetylene black, furnace black, channel black, ultra-high carbon black and combinations thereof.

7. The composition for preparing an anti-slip film according to claim 5, characterized in that: The carbon nanotubes are bundled carbon nanotubes with an average bundle diameter of 0.5 μm to 20 μm, an average bundle length of 10 μm to 200 μm, and an apparent density of 0.005 g / mL to 0.120 g / mL.

8. The composition for preparing an anti-slip film according to claim 1 or 2, characterized in that: The conductive component includes conductive carbon black and carbon nanotubes in a weight ratio of 1:1 to 3:

1.

9. A composition for preparing an anti-slip film, characterized in that: Relative to 100 parts by weight of the thermoplastic elastomer other than the olefin elastomer, including: 60 to 90 parts by weight of a tackifier; 20 to 80 parts by weight of an ethylene / α-olefin block copolymer; 15 to 30 parts by weight of an olefin resin; and 20 to 30 parts by weight of a conductive component, The olefin resin is at least one selected from the group consisting of high-density polyethylene resin, low-density polyethylene resin, linear low-density polyethylene resin, polypropylene resin and ethylene-propylene copolymer resin. Also included are polyoctenes.

10. The composition for preparing an anti-slip film according to claim 9, characterized in that: The content of the polyoctenylene is 5 to 20 parts by weight, and the CIS ratio of double bonds is 10% to 30%.

11. A backing paper for transporting a display panel, characterized in that: include: Foam sheets; and An anti-slip film is formed on at least one side of the foam sheet. The anti-slip film includes a cured product of the composition according to any one of claims 1 , 2 , 9 and 10 .

12. The backing paper for transporting a display panel according to claim 11, characterized in that: The foam sheet is one selected from the group consisting of polyethylene, polypropylene, ethylene vinyl acetate, polyurethane and a combination thereof.