A method for preparing composite copper foil
By growing a zinc oxide nanofilm on a polymer base film and loading precious metal nanoparticles, and using electroless copper plating method to prepare composite copper foil, it solves the problems of expensive equipment and poor adhesion in the existing process, and achieves high adhesion. and improved electrical conductivity, suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202311709934.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-13
AI Technical Summary
The existing composite copper foil preparation process has problems such as expensive equipment, complex processes, poor adhesion and low material safety, which especially affects battery performance and safety in lithium batteries.
Spray baking method is used to grow zinc oxide nanofilm on the polymer base film, and precious metal nanoparticles are loaded on the surface. Composite copper foil is prepared through electroless copper plating method, which simplifies the process and improves the adhesion between the copper foil and the substrate.
It achieves high adhesion and conductive properties of the composite copper foil, reduces equipment costs, simplifies the process, is suitable for large-scale industrial production, and improves the performance and safety of lithium batteries.
Smart Images

Figure BDA0004604394550000091 
Figure BDA0004604394550000101 
Figure BDA0004604394550000102
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal film preparation, and relates to a method for preparing a composite copper foil. Background Art
[0002] As the "current collector" of lithium-ion batteries, the quality of copper foil determines the energy density, battery capacity and cycle life of lithium batteries. High safety and high specific energy are the development trends of lithium battery copper foil in the future. Composite copper foil is composed of insulating polymer materials such as PET (polyethylene terephthalate) and PP (polypropylene) as the base material, and copper foil layers covering the upper and lower surfaces. Composite copper foil adopts a "sandwich" structure. With its unique polymer material, it solves the problem of thermal runaway caused by short circuits in batteries, while increasing the battery energy density by 5-10% and the cycle life by 5%. Composite copper foil has the advantages of thin thickness, low copper consumption, good compatibility, high safety, and high energy density. The scale of the industry will continue to expand in the future. Lithium battery copper foil is developing in the direction of lightness, high density, high tensile strength and high elongation.
[0003] The current production process of composite copper foil mainly includes a one-step water electroplating, a two-step process of magnetron sputtering priming and water electroplating thickening, and a one-step process of magnetron sputtering. Chinese invention patent application CN115700295A discloses a continuous preparation process of PET composite copper foil, which uses PET as a carrier, deposits a uniform thin copper layer on the surface by magnetron sputtering, and then increases the thickness of the PET composite copper foil by pulse electroplating. The base composite structure of Cu-PET-Cu is adopted, and the preparation process is stable and controllable, with a thickness of more than 10μm.
[0004] Chinese invention patent application CN115058711A discloses a method for preparing an ultra-thin carrier copper foil that is easy to peel off. The ultra-thin carrier copper foil includes a carrier copper foil layer, a peeling layer, and an ultra-thin copper foil layer. The peeling layer includes a metal layer and an organic layer. The metal layer is obtained by magnetron sputtering an amorphous alloy of Fe, B, Co, and Ni, and the organic layer is obtained by adsorption treatment of an organic liquid containing nitrogen-containing organic matter, thereby forming a composite peeling layer with uniform surface and stable performance on the upper surface of the copper foil. The carrier foil that has been adsorbed is immersed in an electroplating copper solution to prepare the ultra-thin copper foil by electrodeposition.
[0005] Due to the large crystallinity, small polarity and low surface energy of the non-metallic polymer substrate, the adhesion between the coating and the substrate will be affected during sputtering and evaporation, and the polymer substrate is a non-conductive insulator and cannot be thickened by electroplating. Therefore, it is necessary to first perform surface activation treatment to form a conductive metal film, and then perform an electroplating thickening process. However, the equipment required for the electroplating process is all large precision instruments, and the magnetron sputtering target consumes a lot of electricity, the evaporation consumes a lot of electricity, and the subsequent water electroplating yield is difficult to control. Therefore, this method has high equipment cost and high process difficulty. In addition, vacuum evaporation and water electroplating cause the material to easily form large breakdown holes and pinholes, which not only affects the battery production process, but also affects the safety of lithium batteries.
[0006] Chinese invention patent application CN116445996A discloses a current collector composite copper foil and its preparation process, which includes a first electroplated copper layer, a first chemically plated copper layer, a thin film carrier layer, a second chemically plated copper layer and a second electroplated copper layer from bottom to top. The surface roughness of the thin film carrier layer is increased by activation treatment, and the initial plating thickness is increased by chemical plating. On the one hand, the process increases the plating thickness, increases the conductivity, reduces the resistance, and can increase the subsequent electroplating efficiency. On the other hand, the bonding force between the chemically plated layer and the thin film carrier layer is increased by roughening the surface of the thin film carrier, and the copper foil layer of the composite copper foil finally formed has a greater bonding force. However, there is still a complex process of electroplating, and the thin film carrier layer needs to be roughened to achieve the improvement of bonding force, which also increases the process flow. In addition, although the increase in the plating thickness increases the conductivity, it is contrary to the direction of lightweight development of composite copper foil, which limits its application.
[0007] Based on the above-mentioned problems existing in the existing technology, the preparation of lightweight composite copper foil with excellent comprehensive performance still faces great challenges. Simple processes such as chemical plating are expected to replace magnetron sputtering, vacuum sputtering and electroplating processes to realize the industrialization and mass production of composite copper foil. Summary of the invention
[0008] The present invention provides a composite copper foil preparation method to solve the problem of complex process and expensive equipment for magnetron sputtering priming and then water electroplating thickening. The zinc oxide nanofilm is quickly grown on the surface of the base film by spray roasting, which has the characteristics of simple operation and large-scale application, and can improve the adhesion between the copper foil and the base material of the composite copper foil.
[0009] The technical solution of the present invention is as follows:
[0010] A method for preparing a composite copper foil comprises the following steps:
[0011] (1) Preparation of zinc oxide nanolayer: spraying an alcohol solution of zinc salt on a polymer base film, and subjecting the film to heat treatment to obtain a composite film 1;
[0012] (2) Loading precious metal nanoparticles: immersing the composite membrane 1 in a polyol solution containing precious metal salts and stabilizers to reduce the precious metal ions to precious metal nanoparticles, and washing to obtain the composite membrane 2;
[0013] (3) Chemical copper plating: The composite film 2 is immersed in an alkaline chemical copper plating solution for copper plating to obtain a composite copper foil.
[0014] Furthermore, the high molecular polymer base film is selected from at least one of a polyimide (PI) film, a polyethylene terephthalate (PET) film and a polyphenylene sulfide (PPS) film.
[0015] Furthermore, the thickness of the high molecular polymer base film is 1.5-20 μm.
[0016] Furthermore, the alcohol solution of zinc salt comprises zinc salt, nitrogen-containing ligand, dispersing aid and ethanol.
[0017] Furthermore, the zinc salt is selected from ZnSO 4 7H 2 O、ZnCl 2 、Zn(NO 3 ) 2 6H 2 O and Zn (OAC) 2 ·2H 2 O at least one; preferably Zn (OAC) 2 ·2H 2 O.
[0018] Furthermore, the nitrogen-containing ligand is selected from at least one of triethanolamine, diethanolamine, ethanolamine, tripropanolamine and dipropanolamine; preferably ethanolamine.
[0019] Furthermore, the zinc ion concentration in the alcohol solution of the zinc salt is 10-200 mM, preferably 20-50 mM.
[0020] Furthermore, the concentration of the nitrogen-containing ligand is 10-100 mM, preferably 30-50 mM.
[0021] The thickness of the zinc oxide nanolayer prepared by the preparation method of the present invention is 50nm-2μm, preferably 200nm-1μm.
[0022] Furthermore, the noble metal salt is selected from at least one of Pd, Ag, Ru, Pt, Ir and Au salts, specifically at least one of nitrates, chlorides and acetates of the noble metal; preferably AgNO 3 or PdCl 2 .
[0023] Furthermore, the stabilizer is a surfactant or a high molecular polymer, selected from at least one of cetyltrimethylammonium bromide (CTAB), polyacrylamide (PAM) and polyvinylpyrrolidone (PVP); preferably polyvinylpyrrolidone (PVP).
[0024] Furthermore, the polyol is selected from at least one of ethylene glycol, 1,4-butanediol, 1,5-pentanediol, glycerol and diethylene glycol; preferably ethylene glycol.
[0025] This process mainly utilizes the reducing property of ethylene glycol to reduce precious metal ions into nanoparticles at a certain temperature.
[0026] The particle size of the noble metal nanoparticles prepared by the preparation method of the present invention is 10-200nm, preferably 10-100nm.
[0027] Furthermore, the alkaline chemical copper plating solution comprises copper sulfate, a reducing agent and a complexing agent.
[0028] Furthermore, the reducing agent is a dual reducing agent system consisting of dimethylaminoborane (DMAB) and sodium hypophosphite (SHP).
[0029] Furthermore, the complexing agent is disodium ethylenediaminetetraacetate (EDTA-2Na).
[0030] Furthermore, the alkaline chemical copper plating solution contains Cu 2+ The concentration is 5-20g / L.
[0031] Furthermore, the concentration of disodium ethylenediaminetetraacetate (EDTA-2Na) is 10-30 g / L.
[0032] Furthermore, the concentration of dimethylaminoborane (DMAB) is 0.05-5 g / L; the concentration of sodium hypophosphite (SHP) is 5-100 g / L.
[0033] Furthermore, the pH value of the alkaline chemical copper plating solution is 8-10.
[0034] Furthermore, the heat treatment temperature is 200-500° C., and the treatment time is 1-3 hours.
[0035] In the present invention, during the preparation of the zinc oxide layer, the heat treatment temperature is not higher than the lowest tolerable temperature of the polymer film material used.
[0036] In some embodiments of the present invention, when the high molecular polymer is polyimide (PI), the heat treatment temperature is ≤210°C.
[0037] In some embodiments of the present invention, when the high molecular polymer is polyphenylene sulfide (PPS), the heat treatment temperature is ≤280°C.
[0038] Furthermore, the reduction temperature is 110-180° C. and the reduction time is 40 min-16 h.
[0039] Furthermore, the copper plating temperature is 20-100° C., preferably 60-80° C., and the copper plating time is 1 min-2 h, preferably 3 min-1 h.
[0040] Furthermore, the preparation method further comprises: performing anti-oxidation treatment on the composite copper foil.
[0041] Furthermore, the specific operation is: immersing the composite into an anti-oxidation liquid, squeezing out water, and drying.
[0042] Furthermore, the anti-oxidation liquid is a chromium-free and zinc-free passivation liquid, comprising: benzotriazole and benzoic acid.
[0043] Furthermore, the soaking time is 5-10s.
[0044] Furthermore, the drying is carried out by hot air drying at a temperature of 80-120°C.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) The present invention prepares a zinc oxide nanolayer on a polymer base film, which effectively improves the adhesion between the copper foil layer and the polymer layer; adopts a spraying and heating treatment process, while avoiding the use of expensive laser pulse deposition, magnetron sputtering and other equipment, which is low in cost and easier to achieve large-scale preparation and industrial production;
[0047] (2) The polyol reduction method is used to load precious metal nanoparticles as catalysts on the zinc oxide nanolayer, which not only improves the conductive properties, but also provides catalytic sites for subsequent chemical copper plating. It avoids the complex steps of substrate roughening, immersion in precious metal solutions, tin sensitization, and activation required for conventional chemical copper plating, and can further achieve rapid chemical copper plating. DETAILED DESCRIPTION
[0048] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is merely an exemplary description of the scope of the present invention, and those skilled in the art can make various changes and modifications to the present invention based on the disclosed content, which should also fall within the scope of the present invention.
[0049] Example 1
[0050] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 5 μm);
[0051] The preparation process of composite copper foil is as follows:
[0052] (1) Preparation of zinc oxide nanolayer: Take 0.2195g Zn(OAC) 2 ·2H 2 O, put it into 100 mL of ethanol, stir it continuously to dissolve it into a 10 mM zinc acetate alcohol solution; add 0.1832 g of ethanolamine to make its concentration 30 mM; continue to stir for 1 hour to mix the solution evenly; form a layer of zinc acetate sol on the PET film by spraying, and heat treat it at 200°C for 2 hours to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0053] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0054] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0055] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0056] Example 2
[0057] A composite copper foil, comprising a high molecular polymer layer, a zinc oxide nanolayer containing silver nanoparticles located on both sides of the high molecular polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer containing silver nanoparticles away from the high molecular polymer layer (wherein the high molecular polymer layer is polyimide PI with a thickness of 5 μm);
[0058] The preparation process of composite copper foil is as follows:
[0059] (1) Preparation of zinc oxide nanolayer: Preparation of zinc oxide nanolayer: Take 0.2876g ZnSO 4 7H 2 O, put it into 100mL of ethanol, stir and dissolve it to prepare a 10mM zinc acetate alcohol solution; add 0.3053g of ethanolamine to make its concentration 50mM; continue to stir for 1h to mix the solution evenly; form a layer of zinc acetate sol on the PI film by spraying, and heat treat it at 300℃ for 2h to obtain a PI film with a zinc oxide nanolayer on the surface (i.e., ZnO-PI-ZnO film);
[0060] (2) Loading precious metal nanoparticles: 2.5 g of silver nitrate was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a silver nitrate precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared silver nitrate precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 5 to obtain an ethylene glycol solution of silver nitrate; the ZnO-PI-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PI-ZnO film loaded with precious metal silver nanoparticles (i.e., Ag-ZnO-PI-ZnO-Ag film);
[0061] (3) Chemical copper plating: before copper plating, the Ag-ZnO-PI-ZnO-Ag film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Ag-ZnO-PI-ZnO-Ag film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 h to obtain a composite copper foil;
[0062] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0063] Example 3
[0064] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer containing palladium nanoparticles located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer containing palladium nanoparticles away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 4.5 μm);
[0065] The preparation process of composite copper foil is as follows:
[0066] (1) Preparation of zinc oxide nanolayer: Take 2.195g Zn(OAC) 2 ·2H 2 O, put it into 100mL of ethanol, stir it continuously to dissolve it into a 100mM zinc acetate alcohol solution; add 0.3154g of diethanolamine to make its concentration 30mM; continue to stir for 1h to mix the solution evenly; form a layer of zinc acetate sol on the PET film by spraying, and heat treat it at 200℃ for 2h to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0067] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, and 20 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0068] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0069] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0070] Example 4
[0071] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 6 μm);
[0072] The preparation process of composite copper foil is as follows:
[0073] (1) Preparation of zinc oxide nanolayer: 0.6815 g ZnCl 2 , put it into 100 mL of ethanol, stir and dissolve it to prepare a 50 mM zinc acetate alcohol solution; add 0.1832 g of ethanolamine to make its concentration 30 mM; continue to stir for 1 hour to mix the solution evenly; form a layer of zinc acetate sol on the PET film by spraying, and heat treat it at 200°C for 2 hours to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0074] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 10 mL of the prepared palladium chloride precursor solution was slowly injected, and PAM was added so that PAM / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0075] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0076] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0077] Example 5
[0078] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 5 μm);
[0079] The preparation process of composite copper foil is as follows:
[0080] (1) Preparation of zinc oxide nanolayer: Take 0.2195g Zn(OAC) 2 ·2H 2 O, put it into 100 mL of ethanol, stir it continuously to dissolve it into a 10 mM zinc acetate alcohol solution; add 0.1832 g of ethanolamine to make its concentration 30 mM; continue to stir for 1 hour to mix the solution evenly; form a layer of zinc acetate sol on the PET film by spraying, and heat treat it at 200°C for 1 hour to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0081] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 180° C. for 4 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0082] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 60° C. for 5 min to obtain a composite copper foil;
[0083] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0084] Example 6
[0085] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer away from the polymer layer (wherein the polymer layer is polyphenylene sulfide (PPS) with a thickness of 5 μm);
[0086] The preparation process of composite copper foil is as follows:
[0087] (1) Preparation of zinc oxide nanolayer: Take 0.2195g Zn(OAC) 2 ·2H 2 O, put it into 100mL of ethanol, stir it continuously to dissolve it into a 10mM zinc acetate alcohol solution; add 0.1832g of ethanolamine to make its concentration 30mM; stir it continuously for 1h to mix the solution evenly; form a layer of zinc acetate sol on the PET film by spraying, and heat treat it at 500℃ for 3h to obtain a PPS film with a zinc oxide nanolayer on the surface (i.e., ZnO-PPS-ZnO film);
[0088] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PPS-ZnO film was immersed in the solution, and heated at 110° C. for 40 min to obtain a ZnO-PPS-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PPS-ZnO-Pd film);
[0089] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PPS-ZnO-Pd film is cleaned with ethanol for 3-4 times; 1 g of copper sulfate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na are added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PPS-ZnO-Pd film is immersed in the alkaline chemical copper plating solution, and copper is plated at 100° C. for 2 h to obtain a composite copper foil;
[0090] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0091] Comparative Example 1
[0092] Compared with Example 1, the only difference is that: no zinc oxide layer is included;
[0093] (1) Coarsening: prepare KOH 30g / L+KMnO 4 20g / L alkaline roughening solution, treated at 70℃ for 10min, to etch nanopores on the surface of the base film;
[0094] (2) Neutralization: 3g / 100L acetic acid aqueous solution, soak for 5min;
[0095] (3) Sensitization: immersion in stannous chloride solution, SnCl 2 15g / L, add 4mL of concentrated hydrochloric acid, and soak for 5min at room temperature;
[0096] (4) Pd loading: PdCl 2 Dissolve 0.125 g in 5 mL of concentrated hydrochloric acid, dilute to 250 mL with deionized water, and immerse the above-treated base membrane in it for 5 minutes.
[0097] Comparative Example 2
[0098] Compared with Example 1, the only difference is that the zinc oxide layer does not carry precious metal nanoparticles.
[0099] Comparative Example 3
[0100] Compared with Example 1, the only difference is that: the zinc oxide nanolayer containing palladium nanoparticles is replaced by a zinc oxide nanolayer containing copper nanoparticles;
[0101] The specific operation of step (2) loading copper nanoparticles is as follows:
[0102] 2.9914 g of copper nitrate trihydrate (Cu 2+ Concentration 0.02M), 92g glycerol (concentration 1M), 0.3g PVP-K30 (PVP-K30 / Cu mass ratio = 1:5) and 4g NaOH are mixed, heated to 140°C with stirring, and maintained for 17min to obtain.
[0103] The other steps are the same as in Example 1.
[0104] Comparative Example 4
[0105] Compared with Example 1, the only difference is that 4 mL of the prepared palladium chloride precursor solution is injected.
[0106] Comparative Example 5
[0107] Compared with Example 1, the only difference is that 25 mL of the prepared palladium chloride precursor solution is injected.
[0108] Comparative Example 6
[0109] Compared with Example 1, the only difference is that 4.829g Zn(OAC)2 ·2H 2 O, put into 100 mL of ethanol to obtain 220 mM zinc acetate alcohol solution.
[0110] Comparative Example 7
[0111] Compared with Example 1, the only difference is that 0.1098g Zn(OAC) 2 ·2H 2 O, put into 100 mL of ethanol to obtain a 5 mM zinc acetate alcohol solution.
[0112] Composite copper foil performance test:
[0113] (1) The thickness of the copper foil layer of the composite copper foil prepared in the above-mentioned embodiment and comparative example was tested using a step profiler.
[0114] (2) The adhesion between the film layer and the substrate is tested by the 100-grid method. The adhesion between the copper foil and the substrate is divided into 1-5B levels (as shown in Table 1) with reference to GB / T9286-2021 "Scratching test for paint and varnish films". The general process is: use a multi-blade cutting knife to make 6 parallel cuts on the surface of the material with a spacing of 2 mm.
[0115] Table 1 Bonding strength between copper foil and substrate
[0116]
[0117]
[0118] The performance characterization results of the composite copper foil prepared in the comparative examples of each embodiment are shown in Table 2.
[0119] Table 2 Composite copper foil performance characterization results
[0120]
[0121] It can be seen from the above table that the composite copper foil with the zinc oxide layer has a significantly improved bonding force between the copper layer and the base film compared to the composite copper foil without the layer, which improves the processing performance of the composite copper foil; at the same time, it is helpful to improve the thickness uniformity of the copper foil layer obtained by chemical copper plating in the later stage; it can be seen from the comparison between Examples 2 and 3 and Example 1 that the addition of precious metal particles improves the electrical conductivity and provides catalytic sites for chemical copper plating in the later stage. After replacing with non-precious metal copper, the conductivity is improved, but it is far less than the effect of loading precious metal particles, and it also has a certain impact on the thickness uniformity of the copper foil; the effect on the adhesion of the composite copper foil is the same; compared with Example 1, when the load of the precious metal is too high, the dispersion of the comparative examples 4 and 5 is uneven, resulting in a certain degree of decrease in adhesion and thickness uniformity. If it is too low, the copper plating efficiency will be low, and the ability to improve adhesion is insufficient, which cannot meet the needs of chemical copper plating in the later stage; compared with Example 1, if the zinc oxide layer is too thick, it is not conducive to chemical copper plating in the later stage, resulting in a significant decrease in the thickness uniformity of the copper foil layer, and the adhesion of the copper layer is reduced, while the oxide layer is too thin, and the adhesion of the composite copper foil cannot be better improved.
[0122] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a composite copper foil, characterized in that: The steps include: (1) Preparation of zinc oxide nanolayer: spraying an alcohol solution of zinc salt on a polymer base film, and subjecting the film to heat treatment to obtain a composite film 1; (2) Loading precious metal nanoparticles: immersing the composite membrane 1 in a polyol solution containing precious metal salts and stabilizers to reduce the precious metal ions to precious metal nanoparticles, and washing to obtain the composite membrane 2; (3) Chemical copper plating: immersing the composite film 2 in an alkaline chemical copper plating solution for copper plating to obtain a composite copper foil; The alcohol solution of the zinc salt comprises a zinc salt, a nitrogen-containing ligand and ethanol; the zinc salt is selected from at least one of ZnSO4·7H2O, ZnCl2, Zn(NO3)2·6H2O and Zn(OAC)2·2H2O; the nitrogen-containing ligand is selected from at least one of triethanolamine, diethanolamine, ethanolamine, tripropanolamine and dipropanolamine; The zinc ion concentration in the alcohol solution of the zinc salt is 10-200 mM; The alkaline chemical copper plating solution comprises copper sulfate, a reducing agent and a complexing agent; the reducing agent is a dual reducing agent system consisting of dimethylaminoborane and sodium hypophosphite; the complexing agent is disodium ethylenediaminetetraacetate; Cu 2+ The concentration is 5-20g / L, the concentration of sodium hypophosphite is 5-100g / L, the concentration of dimethylaminoborane is 0.05-5g / L; the concentration of disodium ethylenediaminetetraacetate is 10-30g / L; The thickness of the zinc oxide nanolayer is 50nm-2μm.
2. The preparation method according to claim 1, characterized in that: The concentration of the nitrogen-containing ligand is 10-100 mM.
3. The preparation method according to claim 1, characterized in that: The noble metal salt is selected from at least one of Pd, Ag, Ru, Pt, Ir and Au salts; the stabilizer is selected from at least one of cetyltrimethylammonium bromide, polyacrylamide and polyvinylpyrrolidone (PVP); and the polyol is selected from at least one of ethylene glycol, 1,4-butanediol, 1,5-pentanediol, propylene glycol and diethylene glycol.
4. The preparation method according to claim 3, characterized in that: The noble metal salt is at least one of nitrate, chloride and acetate of the noble metal.
5. The preparation method according to claim 1, characterized in that: The pH value of the alkaline chemical copper plating solution is 8-10.
6. The preparation method according to claim 1, characterized in that: The heat treatment temperature is 200-500° C., and the heat treatment time is 1-3 hours; the reduction temperature is 110-180° C., and the reduction time is 40 minutes to 16 hours; the copper plating temperature is 20-100° C., and the copper plating time is 1 minute to 2 hours.
7. The preparation method according to claim 6, characterized in that: The copper plating temperature is 60-80° C., and the copper plating time is 3 min-1 h.
8. The preparation method according to claim 1, characterized in that: Also includes: The composite copper foil is subjected to anti-oxidation treatment; the specific operation is: immersing the composite foil in an anti-oxidation solution, squeezing out water, and drying.
9. The preparation method according to claim 8, characterized in that: The anti-oxidation liquid is a chromium-free and zinc-free passivation liquid, which includes benzotriazole and benzoic acid.
Citation Information
Cited By
Preparation method and application of lithium-philic composite copper current collector
CN120280494A