A method for preparing porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries
By using the preparation method of porous SiO@C structure in lithium-ion batteries, the stability and disproportionation reaction problems of silicon oxide are solved, and the battery performance with high capacity and cycle stability is achieved. By using alcohol in lithium-ion batteries, Materials such as deionized water and hydrochloric acid form a porous structure and are coated with carbon at high temperatures, avoiding the formation of silica and improving the electrochemical properties of the battery.
Patent Information
- Application Number
- CN202311097722.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-08-29
AI Technical Summary
In the prior art, silicon oxide is difficult to store stably and easily agglomerate, and disproportionate reactions are prone to occur when preparing SiO@C structures, resulting in poor conductivity and low electrochemical performance.
Using a preparation method of porous SiO@C for silicon carbon anode material for lithium-ion batteries, monomethyltrimethoxysilane, silicate and cetyltrimethyl Basic ammonium bromide forms a sol, then mixes with pretreated silicon powder, gel, aging, drying and ball milling, then heated under an inert atmosphere and introduced into acetylene to form a porous SiO@C structure to avoid high temperature disproportionation reaction .
Effectively solve the stability problem of sub-silicon oxide, improve the specific capacity and cycle stability of the battery, the first effect reaches more than 90%, and the high capacity remains after 200 cycles of charging and discharging, reducing the expansion effect after lithium embedded, and improving electronic migration efficiency.
Smart Images

Figure CN117727882B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a method for preparing porous SiO@C, a silicon-carbon negative electrode material for lithium-ion batteries. Background Art
[0002] With the rise of new energy electric vehicles, people have an increasing demand for high-capacity lithium-ion batteries. However, the theoretical specific capacity of traditional graphite electrodes is only 372mAh / g, which can no longer meet the needs of society. High-capacity batteries are in urgent need of development. Silicon-based materials are receiving more and more attention due to their high theoretical specific capacity of 4200mAh / g. Silicon-based materials do not have the risk of lithium precipitation and are safer than graphite-based negative electrode materials. In addition, silicon-based materials can provide channels for lithium ion embedding and extraction from all directions, and have excellent fast charging performance, which is suitable for the current era's pursuit of power batteries.
[0003] However, silicon-based materials have high volume expansion (300%-400%) and serious interface side reactions during the insertion and extraction of lithium, which limits their further development. The existing technology solves this problem by nano-sizing and making silicon-based materials porous, preparing silicon oxide or carbon coating. Compared with pure silicon powder, silicon oxide has a smaller volume effect during the charge and discharge process, better cycle performance, and a lower voltage platform, while maintaining a high specific capacity of 2000mAh / g. However, silicon oxide produced by traditional methods is unstable and easy to agglomerate, and it is easy to undergo disproportionation reaction to generate silicon and silicon dioxide at room temperature. Because of the presence of silicon dioxide, the performance of silicon oxide will be reduced to a certain extent. Through carbon coating technology, silicon oxide is isolated from the outside world in a high-temperature inert gas atmosphere, so that the performance of silicon oxide can be stabilized, and the carbon-coated silicon oxide structure can effectively reduce side reactions, reduce the internal friction of the electrolyte, and is conducive to the conduction of lithium ions in the negative electrode active material.
[0004] CN114464785A discloses a method for preparing a carbon-coated silicon oxide negative electrode material, the preparation steps of which are: firstly, carbon is deposited on the surface of silicon oxide by a low-temperature CVD gas phase method, and then high-temperature disproportionation is performed to obtain a carbon-coated silicon oxide negative electrode material. This method solves the problem that silicon oxide is unstable and easily undergoes disproportionation reaction at room temperature to generate silicon and silicon dioxide. However, the preparation method uses SiO finished product and directly performs carbon coating, and the reaction process involves disproportionation reaction, which converts part of SiO into +4 valence SiO 2 , which will essentially reduce the conductivity of the product and weaken the electrochemical properties of the electrode material. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing porous SiO@C, a silicon-carbon negative electrode material for lithium-ion batteries, to solve the problems that silicon monoxide is difficult to store stably and is easy to agglomerate, and that when the SiO@C structure is prepared by the existing method, a disproportionation reaction is easily generated to form silicon dioxide, resulting in poor conductivity and low electrochemical performance of the obtained battery.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries comprises the following steps:
[0008] S1. Evenly mix alcohol, deionized water and hydrochloric acid to obtain a mixed solution A; evenly mix monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane and hexadecyltrimethylammonium bromide to obtain a mixed solution B; evenly mix the mixed solution A and the mixed solution B, and hydrolyze them at a temperature of 50 to 60° C. for 3 to 5 hours to obtain a sol;
[0009] S2. Add the pretreated silicon powder to the sol obtained in step S1, mix well, and then perform gelation, aging, drying, and ball milling in sequence to obtain porous aerogel coated powder; the pretreatments are ball milling, screening, and demagnetization in sequence.
[0010] S3, adding the porous aerogel coated powder obtained in step S2 into a reaction device at 1300-1400° C. under an inert atmosphere, continuing to heat to 1400-1600° C., keeping the temperature for 1-4 hours; then cooling to 700-900° C.;
[0011] The inert atmosphere is argon or nitrogen. When feeding, the temperature of the reaction device is controlled at 1300-1400°C because the material is added after the temperature rises to 1300°C, which can prevent the powder from sticking to the wall and hindering the reaction. Controlling the reaction temperature above 1400°C can make the reaction faster and more thorough, and controlling the reaction temperature below 1600°C is to reduce the requirements for equipment and thus reduce costs.
[0012] S4, introducing acetylene into the product obtained in step S3, and reacting at 700-900° C. for 2-4 hours; after cooling, the obtained powder is porous SiO@C, a silicon-carbon negative electrode material.
[0013] Furthermore, in step S1, the hydrochloric acid is 0.1M dilute hydrochloric acid; the volume ratio of alcohol, deionized water, and hydrochloric acid is 10-20:5-15:0.5-1; the mass ratio of monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane, and hexadecyltrimethylammonium bromide is: 2-8:1-5:0-1:0-1; the volume mass ratio of mixed solution A and mixed solution B is: 15.5-36ml: 3.5g-15g. The aerogel produced in this range is more flexible and stronger. That is, the aerogel has a larger pore size, so that when preparing porous silicon oxide, the porous structure of silicon oxide can be better maintained, and more space is reserved for the expansion of silicon after lithium insertion, which enhances the cycle stability of the battery. In addition, the porous structure of large-pore aerogel can increase the contact area with silicon powder, increase the generation rate of silicon oxide, and improve the reaction efficiency.
[0014] Furthermore, in step S1, the hydrochloric acid is 0.1M dilute hydrochloric acid; the volume ratio of alcohol, deionized water, and hydrochloric acid is 12:9:0.8; the mass ratio of monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane, and hexadecyltrimethylammonium bromide is 5:4:0.5:0.5; and the volume mass ratio of mixed solution A and mixed solution B is 21.8ml:10g.
[0015] Furthermore, in step S2, the molar ratio of silicon powder to silicon element in the sol is 1:1. This makes it easier for silicon dioxide in the sol to completely react to generate silicon monoxide.
[0016] Furthermore, the particle size of the silicon powder after pretreatment is 500nm to 1μm. The present invention uses silicon powder with a larger particle size as raw material, which can save the preparation cost. The particle size of the silicon powder after pretreatment is preferably 500nm.
[0017] Furthermore, the gelation, aging, drying, and ball milling are specifically as follows: first prepare 1-2M ammonia water, then add the ammonia water to the mixed sol obtained in step S2, and gel for 2-5 minutes; then soak the obtained gel in methanol for 7-10 hours for aging, then dry it in an environment of 120-140°C for 3-5 hours or use supercritical carbon dioxide technology to dry it for 4-6 hours, and then use a ball mill to crush the dried block to less than 10um. The volume ratio of the ammonia water to the mixed sol is 2-5ml ammonia water: 30ml sol.
[0018] Furthermore, the reaction device in step S3 is a heating rotary kiln, which has low requirements on equipment and is suitable for large-scale application.
[0019] Furthermore, after the silicon powder is demagnetized, the iron element accounts for 0.01-1wt% and the remainder is silicon powder. The silicon powder used in the present invention is silicon powder waste, which has a low cost, and the silicon powder contains a small amount of iron compounds, which can inhibit the volume expansion of the silicon-carbon negative electrode and enhance the cycle stability.
[0020] Furthermore, in step S1, the alcohol is methanol or ethanol; and the silicate is methyl silicate or ethyl silicate.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention effectively solves the problem of the difficulty in stably preserving silicon oxide by carbon coating the prepared silicon oxide. In the process of carbon coating, the waste heat of the high-temperature neutralization reaction is directly used to react, which reduces energy loss and can prevent the silicon oxide generated by the high-temperature neutralization reaction from contacting the air, thereby effectively preventing the silicon oxide from being reoxidized to silicon dioxide, causing the material to fail. The battery made of the silicon-carbon negative electrode material of the present invention has a high specific capacity, and the first efficiency can reach more than 90%. After 200 cycles of charge and discharge, it still maintains a high capacity retention rate and has good cycle stability.
[0023] 2. The method for preparing the silicon-carbon negative electrode material of the present invention uses a large-pore aerogel as a precursor to prepare a porous silicon-oxygen material, which can improve the efficiency of electron migration, reduce the negative impact of silicon expansion, and maintain the stability of the charge and discharge cycle; and the large-pore aerogel has a large number of pores, which can increase the contact area with silicon powder, increase the generation rate of silicon oxide, and improve the reaction efficiency. In addition, the silicon-carbon negative electrode material prepared by the method of the present invention is loose and porous, which can more effectively reduce the negative impact of the expansion problem after lithium insertion.
[0024] 3. The large-pore silicon-based aerogel precursor used in the present invention has an amorphous structure. Compared with conventional SiO 2 It is easier to convert, has a lower reaction temperature, lower equipment requirements, and higher conversion efficiency. In addition, the porous silica powder is easier to maintain in powder form during the conversion process, reducing the incomplete coating and structural damage caused by agglomeration. The silicon powder used is silicon powder waste, which has a lower cost, and the silicon powder contains a small amount of iron compounds, which can inhibit the volume expansion of the silicon-carbon negative electrode and enhance the cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the coating structure of the silicon-carbon negative electrode material of the present invention. DETAILED DESCRIPTION
[0026] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.
[0027] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0028] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.
[0029] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.
[0030] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods.
[0031] The quantitative tests in the present invention were repeated three times and the results were averaged.
[0032] Note: The silicon powder described in the present invention is all silicon powder waste. After demagnetization, the iron element accounts for 0.01-1wt% and the rest is silicon powder.
[0033] Example 1
[0034] A method for preparing porous SiO@C, a silicon-carbon negative electrode material for lithium-ion batteries, comprising the following steps:
[0035] S1: Glue preparation: 300 ml of methanol, 150 ml of deionized water, and 10 ml of 0.1 M dilute hydrochloric acid are mixed to form a mixed solution A; 100 g of monomethyltrimethoxysilane (MTMS), 80 g of methyl silicate (TMOS), 10 g of dimethyldimethoxysilane (DMDMS), and 1 g of hexadecyltrimethylammonium bromide (CTAB) are mixed to form a mixed solution B; after mixing the mixed solutions A and B, stir at 55°C for 4 h to obtain a sol;
[0036] S2: Mixed silicon powder: Take 37 g of silicon powder, and after ball milling, screening, demagnetization and other processes, add the obtained silicon powder into the prepared sol, stir with a stirring paddle to obtain a mixed sol.
[0037] S3: Gel aging: Prepare 1.5M ammonia water, add the ammonia water to the mixed sol described in S2, and gel for 4 minutes. After gelation, add methanol to the obtained gel, soak and age for 8 hours to obtain a large-pore aerogel (SiO 2 )A block of silicon powder structure coated.
[0038] S4: Drying and ball milling: The aged block is placed in an environment of 120° C. for drying for 4 hours. After drying, the block is crushed into pieces less than 10 μm using a ball mill to obtain porous aerogel powder.
[0039] S5: High temperature return: Heat the rotary kiln, continue to introduce argon gas to replace the gas in the furnace tube, and add the porous aerogel powder obtained in step S4 at 1300°C, continue to heat to 1500°C, stop introducing argon gas, and maintain for 2 hours. After the temperature starts to drop, continue to introduce argon gas until the temperature drops to 900°C to obtain porous SiO.
[0040] S6: Gas phase carbon coating: stop the injection of argon / nitrogen, start injecting acetylene, and keep the temperature at 900°C for 2h.
[0041] S7: After the temperature drops to room temperature, porous SiO@C, a silicon-carbon negative electrode material, is obtained.
[0042] Through transmission electron microscopy observation, we can see that its structural diagram is as follows Figure 1 shown.
[0043] Example 2
[0044] A method for preparing porous SiO@C, a silicon-carbon negative electrode material for lithium-ion batteries, comprising the following steps:
[0045] S1: Glue preparation: 180 ml of methanol, 90 ml of deionized water, and 10 ml of 0.1 M dilute hydrochloric acid are mixed and called mixed solution A; 100 g of monomethyltrimethoxysilane (MTMS), 20 g of methyl silicate (TMOS), and 1 g of dimethyldimethoxysilane (DMDMS) are mixed and called mixed solution B; after mixing mixed solutions A and B, stir at 55° C. for 4 h to obtain a sol;
[0046] S2: Mixed silicon powder: Take 24.4 g of silicon powder, and after ball milling, screening, demagnetization and other processes, add the obtained silicon powder into the prepared sol, stir with a stirring paddle to obtain a mixed sol.
[0047] S3: Gel aging: Prepare 1.5M ammonia water, add the ammonia water to the mixed sol in S2, and control the gel time to 5 minutes through pre-gel experiment. After gelation, add methanol to the obtained gel, soak and age for 8 hours to obtain a large-pore aerogel (SiO 2 )A block of silicon powder structure coated.
[0048] S4: Drying and ball milling: The aged block is dried for 4 hours using supercritical carbon dioxide technology. After drying, the block is crushed to less than 10 μm using a ball mill to obtain porous aerogel powder.
[0049] S5: High temperature return: Heat the rotary kiln, continue to introduce argon gas to replace the gas in the furnace tube, and add the porous aerogel powder obtained in step S4 at 1400°C, continue to heat to 1600°C, stop introducing argon gas, and maintain for 2 hours. After the temperature starts to drop, continue to introduce argon gas until the temperature drops to 900°C to obtain porous SiO.
[0050] S6: Gas phase carbon coating: stop the injection of argon / nitrogen, start injecting acetylene, and keep the temperature at 900°C for 2h.
[0051] S7: After the temperature drops to room temperature, porous SiO@C, a silicon-carbon negative electrode material, is obtained.
[0052] Through transmission electron microscopy observation, we can see that its structural diagram is as follows Figure 1 shown.
[0053] Application Example A negative electrode sheet for lithium ion battery
[0054] The silicon-carbon negative electrode materials prepared in Examples 1 and 2 are respectively used to prepare electrode sheets, and the specific steps include:
[0055] S1. Grind the silicon-carbon negative electrode material and the conductive agent thoroughly, add the binder, mix thoroughly, and apply it on the copper foil with a thickness of 200μm. The conductive agent is one of acetylene black, Ketjen black, and carbon nanotubes; the binder is one or more of LA133, LA136D, CMC, and SBR. The mass ratio of active material, conductive agent, and binder is 7:2:1; after coating, air dry until the surface is completely solidified and compact it.
[0056] S2. Dry the compacted material in a vacuum environment at 120° C. for 12 h, and cut it as needed to obtain a silicon-carbon negative electrode sheet.
[0057] Comparative Example 1
[0058] CN114464785A discloses a method for preparing a carbon-coated silicon oxide negative electrode material, comprising the following steps:
[0059] Silicon dioxide is placed in a nitrogen-protected CVD reactor, nitrogen is introduced at a nitrogen flow rate of 1.6 L / min, and the temperature is raised to 850°C at a rate of 5°C / min under nitrogen protection, and then ethylene is introduced at a flow rate of 2.45 L / min, and the temperature is kept for 168 minutes. The ethylene is turned off, and the temperature is raised to 1030°C at a rate of 5°C / min, and the high temperature is kept for 2 hours. The temperature is naturally cooled in a nitrogen atmosphere. After the temperature is completely cooled, the material is taken out for screening and depolymerization to obtain a carbon-coated silicon dioxide negative electrode material. This preparation method uses SiO finished products, directly performs carbon coating, and the reaction process involves a disproportionation reaction, which converts part of SiO into +4-valent SiO 2 , which will essentially reduce the conductivity of the product and weaken the electrochemical properties of the electrode material.
[0060] Table 1 Comparison of electrode sheet performances obtained from materials of Examples 1-2 and Comparative Example 1
[0061]
[0062] As shown in Table 1, the battery made of the silicon-carbon negative electrode material of the present invention has a high specific capacity, and the first efficiency can reach more than 90%. After 200 cycles of charge and discharge, it still maintains a high capacity retention rate and good cycle stability. The porous active material more effectively reserves space for the expansion of silicon after lithium insertion. The more complete and uniform carbon coating structure formed by the CVD method reduces the contact between the silicon core and the electrolyte. The combination of the two structures more effectively stabilizes the morphology of the negative electrode material during the charge and discharge process and reduces side reactions, thereby improving the first efficiency and cycle life.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries, characterized in that: The steps include: S1. Evenly mix alcohol, deionized water and hydrochloric acid to obtain a mixed solution A; evenly mix monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane and hexadecyltrimethylammonium bromide to obtain a mixed solution B; evenly mix the mixed solution A and the mixed solution B, and hydrolyze them at a temperature of 50-60° C. for 3-5 hours to obtain a sol; S2, adding the pretreated silicon powder to the sol obtained in step S1, mixing evenly, and then sequentially performing gelation, aging, drying, and ball milling to obtain a porous aerogel coated powder; S3, adding the porous aerogel coated powder obtained in step S2 into a reaction device at 1300-1400°C under an inert atmosphere, continuing to heat to 1400-1600°C, keeping the temperature for 1-4 hours; then cooling to 700-900°C; S4, introducing acetylene into the product obtained in step S3, and reacting at 700-900° C. for 2-4 hours; after cooling, the obtained powder is porous SiO@C, a silicon-carbon negative electrode material; In the step S1, the hydrochloric acid is 0.1M dilute hydrochloric acid; the volume ratio of alcohol, deionized water, and hydrochloric acid is 10-20:5-15:0.5-1; the mass ratio of monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane, and hexadecyltrimethylammonium bromide is 2-8:1-5:0-1:0-1; and the volume mass ratio of the mixed solution A to the mixed solution B is 15.5-36ml:3.5g-15g.
2. The method for preparing the porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: In step S1, the hydrochloric acid is 0.1M dilute hydrochloric acid; the volume ratio of alcohol, deionized water, and hydrochloric acid is 12:9:0.8; the mass ratio of monomethyltrimethoxysilane, silicate, dimethyldimethoxysilane, and hexadecyltrimethylammonium bromide is 5:4:0.5:0.5; and the volume mass ratio of mixed solution A to mixed solution B is 21.8ml:10g.
3. The method for preparing the porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: In the step S2, the molar ratio of silicon powder to silicon element in the sol is 1:
1.
4. The method for preparing the porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: The particle size of silicon powder after pretreatment is 500nm~1μm.
5. The method for preparing the porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: The gelation, aging, drying and ball milling are specifically as follows: first prepare 1-2M ammonia water, then add the ammonia water to the mixed sol obtained in step S2, and gel for 2-5 minutes; then soak the obtained gel in methanol for 7-10 hours for aging, then dry it in an environment of 120-140°C for 3-5 hours or use supercritical carbon dioxide technology to dry it for 4-6 hours, and then use a ball mill to crush the dried block to less than 10um.
6. The method for preparing porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: The reaction device in step S3 is a heating rotary kiln.
7. The method for preparing porous SiO@C silicon-carbon negative electrode material for lithium-ion batteries according to claim 1, characterized in that: After the silicon powder is demagnetized, the iron element accounts for 0.01-1wt% and the remainder is silicon powder.