A luminescent material for optical thermometer with high sensitivity and preparation method thereof

CN117736732BActive Publication Date: 2024-11-15HUAIYIN TEACHERS COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311538382.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-11-15
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

但是这种接触式测量温度的方式,有很大弊端,如果被测样品粒度较小,或者热容量相对于日常所测材料明显较低,在这些场景下,使用接触式测量物体温度,则会产生较大的测量误差

Benefits of technology

[0019] 1. This invention utilizes Y for the first time 30 W 8 O 69 It is a matrix material and is doped with Eu rare earth ions to prepare a luminescent material. The material has stable physical and chemical properties, is not easily affected by an oxygen-containing environment, has excellent luminescent properties, has a simple preparation process, does not produce three wastes, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117736732B_ABST
    Figure CN117736732B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of optical temperature sensing materials, and specifically discloses a luminescent material for an optical thermometer with high sensitivity and a preparation method thereof. The general formula of the luminescent material is shown in the following chemical formula: 30(1‑x) Eu 30x W8O 69 , wherein x is 1% to 30%. The preparation method comprises the following steps: 30(1‑x) Eu 30x W8O 69 The initial raw materials WO3, Y2O3, Eu2O3 and H3BO3 are weighed in the molar ratio of the elements shown, put into an agate mortar, add an appropriate amount of ethanol and grind once to make them evenly mixed, the ground raw materials are first pre-burned in a muffle furnace with a corundum crucible, and after the pre-burning, the sample is taken out after cooling, poured into an agate mortar and H3BO3 is added, and then ethanol is added for grinding again, and finally the ground sample is sintered in a muffle furnace and cooled with the furnace to obtain the final product. The luminescent material provided by the present invention has stable performance and high temperature detection sensitivity, has broad application prospects in the field of optical temperature sensing, and the preparation method is simple to operate, has extremely low requirements on equipment, and has low production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical temperature sensing materials, and in particular relates to a luminescent material for an optical thermometer with high sensitivity and a preparation method thereof. Background Art

[0002] Temperature detection, as an indispensable measurement method, has always been used in people's production monitoring and life detection. The traditional temperature detection method generally adopts a contact measurement method to obtain the measured temperature by temperature conduction. This method is widely used in industry, agriculture, commerce and medical fields. However, this contact temperature measurement method has great disadvantages. If the particle size of the sample to be measured is small, or the heat capacity is significantly lower than that of the material measured in daily life, in these scenarios, the contact measurement of the object temperature will produce a large measurement error. Therefore, researchers have developed a variety of new non-contact measurement methods, such as infrared detection technology, Raman spectroscopy temperature measurement technology, thermal modulation reflectance spectrum technology and fluorescence intensity ratio technology. Among them, the fluorescence intensity ratio technology has a small dependence on measurement conditions and can effectively reduce the temperature measurement errors caused by factors other than temperature, such as air pressure changes, excitation source fluctuations, and fluorescence transmission losses. It is a highly advantageous temperature measurement technology and has attracted widespread attention. Therefore, the up-conversion luminescent materials under this technology are used as optical thermometer materials for temperature detection, which has always been an important research content in the field of temperature detection.

[0003] The luminescent material used in optical thermometers consists of three parts: matrix, activator and sensitizer. The matrix provides a suitable crystal field environment for the doped ions, and generally includes fluorides and oxides. In comparison, fluorides have lower phonon energy, and the oxide matrix has excellent thermal stability, which is very promising in temperature sensing and has become the focus of researchers. The activator, that is, the luminescence center, generally has a rich metastable energy level, and the transition width of electrons between metastable energy levels determines the color of the emitted light.

[0004] When using rare earth-doped luminescent materials for temperature detection, two key issues need to be addressed: one is the luminescent intensity of the material, and the other is the sensitivity of measuring temperature. Luminescent intensity is generally affected by the luminescent matrix. Therefore, in order to increase the luminescent brightness, a suitable matrix should be selected, and the brightness of the phosphor can be changed by adding co-solvents and charge compensators during sintering. The level of measurement sensitivity is generally affected by doped ions and the matrix. To obtain higher temperature measurement sensitivity, it is necessary to explore suitable luminescent matrices and doped ions. Therefore, the development of a luminescent material with high sensitivity and good stability has important driving significance in the field of temperature detection. Summary of the invention

[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide a new luminescent material for an optical thermometer with high sensitivity. The luminescent material of the present invention has high temperature detection sensitivity and good stability. Another object of the present invention is to provide a method for preparing the luminescent material.

[0006] The present invention is achieved through the following technical solutions:

[0007] A luminescent material for an optical thermometer with high sensitivity, the general formula of the luminescent material is shown in the following chemical formula: 30(1-x) Eu 30x W8O 69 , where x is 1%~30%.

[0008] Furthermore, in the chemical formula, x = 1%, 3%, 5%, 10%, 20% or 30%.

[0009] A further improvement of the present invention is:

[0010] A method for preparing a luminescent material for an optical thermometer with high sensitivity comprises the following steps:

[0011] According to chemical formula Y 30(1-x) Eu 30x W8O 69 Initial raw materials WO3, Y2O3, Eu2O3 and H3BO3 are weighed in the molar ratio of elements shown, put into an agate mortar, add appropriate amount of ethanol and grind once to make them evenly mixed, the ground raw materials are first pre-burned in a muffle furnace with a corundum crucible, and after pre-burning, the sample is taken out after cooling, poured into an agate mortar and H3BO3 is added, and then ethanol is added for grinding again, and finally the ground sample is sintered in a muffle furnace and cooled with the furnace to obtain the final product; in the chemical formula, x is 1%~30%.

[0012] Preferably, in the chemical formula, x = 1%, 3%, 5%, 10%, 20% or 30%.

[0013] Furthermore, the purity of WO3 is 99%, the purity of Y2O3 is 99.99%, the purity of Eu2O3 is 99.99%, and the purity of H3BO3 is 99%.

[0014] Furthermore, during the first grinding, the amount of ethanol used is 2-4 mL of ethanol per gram of initial raw material, and the grinding time is 20-40 min.

[0015] Furthermore, the pre-firing temperature is 700° C. to 900° C., and the time is 1 to 3 hours.

[0016] Furthermore, during the re-grinding, the amount of H3BO3 used is 0.5-1.5wt% of the initial raw material, the amount of ethanol used is 2-3mL, and the grinding time is 20-30min.

[0017] Furthermore, the sintering temperature is 1300° C. to 1400° C., and the sintering time is 1 to 3 hours.

[0018] The beneficial effects of the present invention are:

[0019] 1. The present invention utilizes Y for the first time 30 W8O 69 The luminescent material is prepared by using Eu rare earth ions as the matrix material. The material has stable physical and chemical properties, is not easily affected by oxygen-containing environments, has excellent luminescent properties, has a simple preparation process, does not produce three wastes, and is environmentally friendly.

[0020] 2. The present invention prepares Y by doping rare earth ions 30(1-x) Eu 30x W8O 69 Luminescent material, the material can emit light in the red light region under ultraviolet light excitation, with high temperature measurement sensitivity. At a temperature of 498 K, the relative sensitivity of the material is as high as 2.3%K -1 , which has broad application prospects in the field of optical temperature sensing.

[0021] 3. The upconversion luminescent material in the present invention is synthesized by solid phase method and is obtained by burning in air atmosphere, without providing inert gas or reducing atmosphere, and is simple to operate, with extremely low requirements on equipment, low production cost, and stable performance of the synthesized luminescent material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 For sample Y 30(1-x) Eu 30x W8O 69 XRD patterns of (x = 1%, 3%, 5%, 10%, 20%, 30%);

[0023] Figure 2 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) excitation spectrum;

[0024] Figure 3 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 Emission spectrum of excited state;

[0025] Figure 4 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 The emission intensity of the excited state varies with Eu 3+ The relationship curve of doping concentration;

[0026] Figure 5 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 Emission spectrum of D0 excited state;

[0027] Figure 6 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 Emission spectrum of excited state;

[0028] Figure 7 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 Emission spectrum of D0 excited state;

[0029] Figure 8 Originated from 5 D1 and 5 The emission peak intensity ratio of D0 level (I 5D1 / I 5D0 ) as a function of temperature and its linear fitting diagram;

[0030] Fig. 9 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 5%) attenuation curve;

[0031] Fig.10 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) attenuation life vs. temperature;

[0032] Fig.11 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) relative sensitivity versus temperature;

[0033] Fig.12 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) is a comparison chart with some other reported luminescent materials in terms of relative sensitivity. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with specific embodiments.

[0035] Example 1-6: Preparation of Y by high temperature solid phase method 30(1-x) Eu 30x W8O 69 sample.

[0036] According to the raw materials and molar ratios shown in Table 1, the initial raw materials WO3 (purity 99%), Y2O3 (purity 99.99%), Eu2O3 (purity 99.99%) and H3BO3 (purity 99%) were weighed and put into an agate mortar with 2~4mL of ethanol for grinding for 20~40min to make them evenly mixed. The ground raw materials were first pre-sintered at 800℃ in a muffle furnace for 2 hours in a corundum crucible, and the samples were taken out after cooling, poured into an agate mortar, and H3BO3 with a ratio of 1wt% of the initial raw materials was added, and 2~3mL of ethanol was added for grinding. Finally, the ground sample was sintered at 1350℃ in a muffle furnace for 2 hours and then cooled in the furnace to obtain the final product.

[0037] Table 1 Expression of samples from Examples 1 to 6

[0038] Serial number x expression Example 1 1% <![CDATA[Y 29.7 I 0.3 W8O 69 ]]> Example 2 3% <![CDATA[Y 29.1 I 0.9 W8O 69 ]]> Example 3 5% <![CDATA[Y 28.5 I 1.5 W8O 69 ]]> Example 4 10% <![CDATA[Y 27 Eu3W8O 69 ]]> Example 5 20% <![CDATA[Y 24 Eu6W8O 69 ]]> Example 6 30% <![CDATA[Y 21 8W 69 ]]>

[0039] In order to verify the performance of the luminescent material prepared by the present invention, the following tests were carried out on the samples prepared in Examples 1 to 6: The physical phase of the samples was detected by an ARL X'TRA X-ray powder diffractometer, the working conditions were 40KV / 35mA, the X-ray generator used CuKα, the wavelength of the ray beam was 1.5418Å, the scanning step was 0.02°, and the scanning range was 10~80°. The luminescence spectrum was measured by a spectrofluorometer system (EI-FS5) of the British Edinburgh Company equipped with a 150W xenon lamp. The fluorescence decay curve was measured using a spectrofluorometer system (EI-FS5) of the British Edinburgh Company using a microsecond flash lamp as the excitation light source. The test results are as follows Figures 1 to 12 shown.

[0040] Figure 1 For sample Y 30(1-x) Eu 30x W8O 69 The XRD patterns of (x = 1%, 3%, 5%, 10%, 20%, 30%) are given by Figure 1 It can be seen that the diffraction peaks of all samples are consistent with the standard card (JCPDS#15-0559), proving that the prepared samples are single-phase and no impure substances are present.

[0041] Figure 2 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) excitation spectrum, given by Figure 2 It can be seen that the strongest excitation peak of the sample is located at 392nm, indicating that the sample can be excited by a near-ultraviolet light source.

[0042] Figure 3 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 The emission spectrum of the excited state is given by Figure 3 It can be seen that the sample has a wavelength of 500~560nm. 5 D 1,2 Four excitation peaks of the excited state.

[0043] Figure 4 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 The emission intensity of the excited state varies with Eu 3+ The relationship between the doping concentration and Figure 4 It can be seen that when Eu 3+ When the doping concentration is 5%, it comes from 5 D 1,2 The excitation peak intensity of the excited state is the largest.

[0044] Figure 5 For sample Y 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 The emission spectrum of the D0 excited state is given by Figure 5It can be seen that the sample has a wavelength of 570-725nm. 5 There are multiple excitation peaks of the D0 excited state, and the strongest peak is located at 625nm.

[0045] Figure 6 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 D 1,2 The emission spectrum of the excited state is given by Figure 6 It can be seen that with the change of temperature, 5 D 1,2 The emission peak intensity of the excited state changes to a certain extent, but the magnitude of the change is not very obvious.

[0046] Figure 7 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 1%, 3%, 5%, 10%, 20%, 30%) is derived from 5 The emission spectrum of the D0 excited state is given by Figure 7 It can be seen that with the increase of temperature, 5 The emission peak intensity of the D0 excited state drops sharply.

[0047] Figure 8 Originated from 5 D1 and 5 The emission peak intensity ratio of D0 level (I 5D1 / I 5D0 ) with temperature and its linear fitting diagram, Figure 8 It can be seen that from 5 The emission peak intensity of the D0 excited state is related to 5 The emission peak intensity ratio of the D1 excited state shows a linear decrease with increasing temperature.

[0048] Fig. 9 is the sample Y at different temperatures 30(1-x) Eu 30x W8O 69 (x = 5%) attenuation curve, given by Fig. 9 It can be seen that with the increase of temperature, 5 The decay time of the emission peak of the D0 excited state changes.

[0049] Fig.10 For sample Y 30(1-x) Eu 30x W8O 69The relationship between the decay life of (x = 5%) and temperature is shown in the figure. Fig.10 It can be seen that from 5 The decay time of the emission peak of the D0 excited state gradually decreases with increasing temperature, which is consistent with Figure 7 The changes in the emission spectra are consistent.

[0050] Fig.11 For sample Y 30(1-x) Eu 30x W8O 69 The relative sensitivity of (x = 5%) varies with temperature, as shown in the figure below. Fig.11 It can be seen that with the increase of temperature, the relative sensitivity of the sample gradually increases. At 498 K, its relative sensitivity reaches 2.3%K. -1 .

[0051] Fig.12 For sample Y 30(1-x) Eu 30x W8O 69 (x = 5%) is compared with some other reported luminescent materials in terms of relative sensitivity. Fig.12 It can be seen that the phosphor material developed in this study has higher sensitivity, indicating that it has potential applications in the field of optical temperature sensing.

[0052] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly sensitive luminescent material for an optical thermometer, characterized in that: The general formula of the luminescent material is shown in the following chemical formula: 30(1-x) Eu 30x W8O 69 , where x is 1%~30%.

2. The luminescent material for an optical thermometer with high sensitivity according to claim 1, characterized in that: In the chemical formula, x = 1%, 3%, 5%, 10%, 20% or 30%.

3. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 1, characterized in that: The following steps are involved: According to chemical formula Y 30(1-x) Eu 30x W8O 69 Initial raw materials WO3, Y2O3, Eu2O3 and H3BO3 are weighed in the molar ratio of elements shown, put into an agate mortar, add appropriate amount of ethanol and grind once to make them evenly mixed, the ground raw materials are first pre-burned in a muffle furnace with a corundum crucible, and after pre-burning, the sample is taken out after cooling, poured into an agate mortar and H3BO3 is added, and then ethanol is added for grinding again, and finally the ground sample is sintered in a muffle furnace and cooled with the furnace to obtain the final product; in the chemical formula, x is 1%~30%.

4. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: In the chemical formula, x = 1%, 3%, 5%, 10%, 20% or 30%.

5. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: The purity of WO3 is 99%, the purity of Y2O3 is 99.99%, the purity of Eu2O3 is 99.99%, and the purity of H3BO3 is 99%.

6. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: During the first grinding, the amount of ethanol used is 2-4 mL of ethanol per gram of initial raw material, and the grinding time is 20-40 min.

7. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: The pre-burning temperature is 700° C. to 900° C., and the pre-burning time is 1 to 3 hours.

8. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: During the re-grinding, the amount of H3BO3 used is 0.5-1.5wt% of the initial raw material, the amount of ethanol used is 2-3mL, and the grinding time is 20-30min.

9. The method for preparing a luminescent material for an optical thermometer with high sensitivity according to claim 3, characterized in that: The sintering temperature is 1300° C. to 1400° C., and the sintering time is 1 to 3 hours.