A method for preparing a boron emitter by PECVD deposition of BSG-boron source layer, and a silicon wafer and device system
By optimizing the PECVD deposition conditions and process flow, the problems of poor boron doping uniformity and difficulty in removing the surface BSG layer on large-sized cells are solved, achieving more efficient boron doping and simplifying the process, which is suitable for large-diameter equipment and improves Production efficiency.
Patent Information
- Application Number
- CN202311783594.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The existing PECVD method of depositing a BSG-boron source layer to prepare boron emitters has problems such as poor boron doping uniformity on large-size cells, difficulty in removing the surface BSG layer, complex processes, and low efficiency, especially in PECVD with large diameters. It is difficult to achieve uniform deposition and efficient doping on equipment.
By optimizing the temperature, pressure and process gas combination of PECVD deposition, combined with silicon wafer pretreatment and thermal annealing treatment, we ensure the full ionization and decomposition of SiH4, B2H6 and N2O, and use diluting gases such as Ar, H2 or N2 to control film color uniformity. , and remove the surface BSG layer through HF solution to simplify the process.
It improves the boron doping uniformity and doping concentration, reduces the difficulty of removing the surface BSG layer, improves the passivation effect, simplifies the process flow, improves production efficiency, and is suitable for large-scale promotion and application.
Smart Images

Figure BDA0004624461650000111 
Figure BDA0004624461650000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells and relates to a method for preparing a boron emitter, and in particular to a method for preparing a boron emitter by depositing a BSG-boron source layer through PECVD, and a silicon wafer and device system. Background Art
[0002] In recent years, the scale of TOPCon battery production has been expanding, and the conversion efficiency has been significantly improved. At present, the mass production efficiency of TOPCon batteries has reached 25.5%, and the laboratory efficiency of some companies has exceeded 26%. In addition, TBC (TOPCon+BC) technology combines TOPCon battery technology and BC battery technology. With the large-scale application of TOPCon technology, TBC battery technology will gradually replace TOPCon battery technology in the next few years and become a new large-scale mass production technology.
[0003] Both TOPCon battery technology and TBC battery technology require the use of a boron source for diffusion doping to prepare a p-type emitter. At present, TOPCon battery mass production uses BBr3 or BCl3 as a boron source for surface doping through thermal diffusion, but there are many problems that have not been solved in this method: (1) B2O3 is easily generated, and B2O3 corrodes quartz devices, which can easily lead to tailpipe blockage. In addition, due to the gravity of B2O3 itself, it is easy to form a square resistance uneven phenomenon after diffusion to the surface of the silicon wafer; (2) Boron diffusion is easy to form a boron-rich layer and winding, which is difficult to clean; (3) Boron has a low solid solubility in silicon and requires high temperature for diffusion. High temperature has high requirements for quartz parts and can easily cause deformation of quartz parts; (4) Traditional boron diffusion is easy to form oxygen rings due to the long high-temperature process time; (5) The route of one boron diffusion + laser SE + secondary boron diffusion (annealing) undergoes two high-temperature treatments, which greatly damages the minority carrier lifetime of the silicon wafer; (6) The process time is long and the production capacity is low.
[0004] In this regard, the method of preparing a boron emitter by PECVD deposition of BSG-boron source layer is expected to replace the method of preparing an emitter by thermal diffusion doping using BBr3 or BCl3 as a boron source. However, this method is currently only used on small-sized batteries. When BSG is deposited on a large-diameter PECVD device for large-sized batteries, the decomposition rate of B2H6 in different regions is often different due to the excessively fast decomposition rate of B2H6, which leads to poor uniformity of boron doping. At the same time, B2H6 has a significant inhibitory effect on the reaction of SiH4 and N2O to generate a-SiOx:B(s). The content of boron atoms in different regions is different, which leads to significant differences in the deposition thickness of a-SiOx:B(s); the difference in the thickness of a-SiOx:B(s) and the mismatch of the ratio of SiH4 to N2O will also result in the inability of the BSG layer on the surface to be removed by HF after annealing.
[0005] It can be seen that how to improve the existing PECVD method of depositing BSG-boron source layer to prepare boron emitter, make it suitable for large-size batteries to deposit BSG on large-diameter PECVD equipment, improve boron doping uniformity and doping concentration, reduce the difficulty of removing the surface BSG layer, improve the passivation effect, simplify the process flow and improve production efficiency, has become a problem that technical personnel in this field urgently need to solve. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer, a silicon wafer and a device system. The method is particularly suitable for depositing BSG on a large-diameter PECVD device for large-size batteries, which improves the uniformity and doping concentration of boron, reduces the difficulty of removing the surface BSG layer, improves the passivation effect, and simplifies the process flow, improves production efficiency, and is conducive to large-scale promotion and application.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer, the method comprising sequentially performing silicon wafer pretreatment, PECVD deposition and thermal annealing.
[0009] Wherein, the temperature of the PECVD deposition is 250-500°C, for example, it can be 250°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C or 500°C, and the pressure is 800-3000mTorr, for example, it can be 800mTorr, 1000mTorr, 1200mTorr, 1400mTorr, 1600mTorr, 1800mTorr, 2000mTorr, 2200mTorr, 2400mTorr, 2600mTorr, 2800mTorr or 3000mTorr, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0010] In the present invention, the temperature and pressure of the PECVD deposition must be strictly controlled within a reasonable range. When the temperature is lower than 250°C, process gases such as SiH4, B2H6 and N2O cannot be fully ionized, which can easily cause abnormal film color and low surface concentration; when the temperature is higher than 500°C, B2H6 decomposes too quickly, which can easily cause uneven film color at the furnace mouth and furnace tail, and most of the B2H6 will gather at the furnace mouth, resulting in a high concentration at the furnace mouth. When the pressure is lower than 800mTorr, the pumping speed of the furnace mouth is too fast, which can easily cause the film color at the furnace mouth to be thin and the concentration to be low; when the pressure is higher than 3000mTorr, there is too much deposition at the furnace mouth, which makes the film thickness at the furnace mouth thicker, and then leads to a high concentration at the furnace mouth.
[0011] In the present invention, the process gas for PECVD deposition includes SiH4, B2H6 and N2O, and the dilution gas includes any one of Ar, H2 or N2 or a combination of at least two of them. Typical but non-limiting combinations include a combination of Ar and H2, a combination of H2 and N2, a combination of Ar and N2, or a combination of Ar, H2 and N2.
[0012] Taking H2 as the diluent gas as an example, during the PECVD deposition process, the reactions that occur on the surface of the pretreated silicon wafer are as follows:
[0013] SiH4(g)+N2O(g)+B2H6(g)+H2(g)→SiO x :B(s)+byproduct
[0014] SiO x :B(s)+high temperature treatment→B doped emitter
[0015] The present invention optimizes and improves the key condition parameters of the existing PECVD method for depositing BSG-boron source layer to prepare a boron emitter, making the method particularly suitable for depositing BSG on a large-diameter (520mm or 540mm) PECVD device for large-size series batteries (182mm series or 210mm series), without significant wrap-around plating, strong process scalability, and not easy to form oxygen rings, thereby improving the uniformity and doping concentration of boron doping, reducing the difficulty of removing the surface BSG layer, and improving the passivation effect. At the same time, the process flow is simplified, the production efficiency is improved, and it is conducive to large-scale promotion and application.
[0016] Preferably, the silicon wafer pretreatment includes: cleaning and texturing the silicon wafer to form a texturing surface on the surface of the silicon wafer; or cleaning and polishing the silicon wafer to form a polishing surface on the surface of the silicon wafer.
[0017] In the present invention, the silicon wafer pretreatment is performed using an alkali solution, such as a KOH solution and / or a NaOH solution.
[0018] Preferably, the PECVD deposition comprises: placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, and the deposition time is 0.1-8000s, for example, it can be 0.1s, 1s, 10s, 100s, 1000s, 2000s, 3000s, 4000s, 5000s, 6000s, 7000s or 8000s, and the power is 5000-30000W, for example, it can be 5000W, 10000W, 15000W, 20000W, 25000W or 30000W. 00W, the pulse switching ratio is 1 / 100-1 / 5, for example, it can be 1 / 100, 1 / 90, 1 / 80, 1 / 70, 1 / 60, 1 / 50, 1 / 40, 1 / 30, 1 / 20, 1 / 10 or 1 / 5, the power frequency is 40-200kHz, for example, it can be 40kHz, 60kHz, 80kHz, 100kHz, 120kHz, 140kHz, 160kHz, 180kHz or 200kHz, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the flow rate of SiH4 in the process gas is 0.1-1slm, for example, it can be 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, and the flow rate of B2H6 is 0.1-1slm, for example, it can be 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm. m, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, the flow rate of N2O is 0.1-1slm, for example, it can be 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Optionally, the dilution gas is only Ar, and the flow rate is 0.01-1slm, for example, it can be 0.01slm, 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Optionally, the dilution gas is only H2, and the flow rate is 0.01-1slm, for example, it can be 0.01slm, 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Optionally, the dilution gas is a combination of Ar and H2, and the flow rate is 0.01-1slm, for example, it can be 0.01slm, 0.1slm, 0.2slm, 0.3slm, 0.4slm, 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm or 1slm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Optionally, the dilution gas is only N2, and the flow rate is 2-10slm, for example, it can be 2slm, 2.5slm, 3slm, 3.5slm, 4slm, 4.5slm, 5slm, 5.5slm, 6slm, 6.5slm, 7slm, 7.5slm, 8slm, 8.5slm, 9slm, 9.5slm or 10slm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the temperature of the thermal annealing treatment is 800-1100°C, for example, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, the time is 10-300min, for example, 10min, 50min, 100min, 150min, 200min, 250min or 300min, and the pressure is 10-1060mbar, for example, 10mbar, 100mbar, 200mbar, 300mbar, 400mbar, 500mbar, 600mbar, 700mbar, 800mbar, 900mbar, 1000mbar or 1060mbar, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, N2 and / or O2 are introduced during the thermal annealing treatment, and the flow rate is 0.01-3slm, for example, it can be 0.01slm, 0.1slm, 0.5slm, 1slm, 1.5slm, 2slm, 2.5slm or 3slm, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, after the thermal annealing treatment, an HF solution is used to remove the BSG layer on the surface of the silicon wafer, and the volume fraction of the HF solution is 15%-80%, for example, it can be 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] As a preferred technical solution of the first aspect of the present invention, the method comprises the following steps:
[0028] (1) cleaning and texturing the silicon wafer to form a velvet surface on the surface of the silicon wafer; or cleaning and polishing the silicon wafer to form a polished surface on the surface of the silicon wafer;
[0029] (2) placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, wherein the deposition temperature is 250-500° C., the pressure is 800-3000 mTorr, the time is 0.1-8000 s, the power is 5000-30000 W, the pulse switch ratio is 1 / 100-1 / 5, the power frequency is 40-200 kHz, the process gas includes 0.1-1 slm SiH4, 0.1-1 slm B2H6 and 0.1-1 slm N2O, and the dilution gas includes any one of 0.01-1 slm Ar, 0.01-1 slm H2 or 2-10 slm N2 or a combination of at least two thereof;
[0030] (3) subjecting the silicon wafer to thermal annealing treatment at a temperature of 800-1100° C., a time of 10-300 min, and a pressure of 10-1060 mbar, and introducing N2 and / or O2 during the thermal annealing treatment at a flow rate of 0.01-3 slm;
[0031] (4) Using HF solution to remove the BSG layer on the surface of the silicon wafer, and the volume fraction of the HF solution is 15%-80%.
[0032] In a second aspect, the present invention provides a silicon wafer, on the surface of which is provided a boron emitter produced by the method described in the first aspect.
[0033] In a third aspect, the present invention provides an apparatus system used in the method as described in the first aspect, wherein the apparatus system comprises a silicon wafer pretreatment unit, a PECVD deposition unit and a thermal annealing unit connected in sequence.
[0034] Preferably, the PECVD deposition unit comprises a PECVD parallel tube.
[0035] Compared with the conventional PECVD single tube, the present invention adopts PECVD parallel tube to deposit the BSG-boron source layer on the silicon wafer surface. This back-to-back design occupies a small area and has high production capacity. The sharing of the electrical system and the vacuum pump reduces the equipment cost and improves the economic benefits.
[0036] In the present invention, the PECVD parallel tubes specifically refer to a device system formed by multiple PECVD furnace tubes arranged in parallel, and the back-to-back design is a design method in which multiple PECVD furnace tubes are arranged in parallel.
[0037] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The present invention optimizes and improves the key condition parameters of the existing PECVD method for depositing BSG-boron source layer to prepare a boron emitter, making the method particularly suitable for depositing BSG on a large-diameter (520mm or 540mm) PECVD device for large-size series batteries (182mm series or 210mm series), without significant wrap-around plating, strong process scalability, and not easy to form oxygen rings, thereby improving the uniformity and doping concentration of boron doping, reducing the difficulty of removing the surface BSG layer, and improving the passivation effect. At the same time, the process flow is simplified, the production efficiency is improved, and it is conducive to large-scale promotion and application. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0041] Example 1
[0042] This embodiment provides a method for preparing a boron emitter by depositing a BSG-boron source layer by PECVD, the method comprising the following steps:
[0043] (1) Using NaOH solution to clean and texturize the silicon wafer to form a velvet surface on the surface of the silicon wafer;
[0044] (2) placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, wherein the deposition temperature is 280° C., the pressure is 2000 mTorr, the time is 4000 s, the power is 18000 W, the pulse switch ratio is 1 / 50, the power frequency is 120 kHz, the process gas includes 0.5 slm SiH4, 0.5 slm B2H6 and 0.5 slm N2O, and the dilution gas is 0.5 slm H2;
[0045] (3) subjecting the silicon wafer to thermal annealing at a temperature of 950° C., a time of 150 min, and a pressure of 500 mbar, with O2 being introduced at a flow rate of 1.5 slm during the thermal annealing process;
[0046] (4) A 50% by volume HF solution is used to remove the BSG layer on the surface of the silicon wafer.
[0047] The device system used in the method provided in this embodiment includes a silicon wafer pretreatment unit, a PECVD deposition unit and a thermal annealing unit connected in sequence, and the PECVD deposition unit includes a PECVD parallel tube. Among them, step (1) is performed in the silicon wafer pretreatment unit, step (2) is performed in the PECVD parallel tube of the PECVD deposition unit, and step (3) is performed in the thermal annealing unit.
[0048] Example 2
[0049] This embodiment provides a method for preparing a boron emitter by depositing a BSG-boron source layer by PECVD, the method comprising the following steps:
[0050] (1) Cleaning and polishing the silicon wafer with a KOH solution to form a polished surface on the surface of the silicon wafer;
[0051] (2) placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, wherein the deposition temperature is 500° C., the pressure is 800 mTorr, the time is 100 s, the power is 30000 W, the pulse switch ratio is 1 / 5, the power frequency is 200 kHz, the process gas includes 0.1 slm SiH4, 1 slm B2H6 and 0.1 slm N2O, and the dilution gas is 0.5 slm H2 and 0.5 slm Ar;
[0052] (3) subjecting the silicon wafer to thermal annealing at a temperature of 1100° C., a time of 100 min, and a pressure of 100 mbar, with N2 being introduced at a flow rate of 1.5 slm during the thermal annealing process;
[0053] (4) A 15% by volume HF solution is used to remove the BSG layer on the surface of the silicon wafer.
[0054] The device system used in the method provided in this embodiment includes a silicon wafer pretreatment unit, a PECVD deposition unit and a thermal annealing unit connected in sequence, and the PECVD deposition unit includes a PECVD parallel tube. Among them, step (1) is performed in the silicon wafer pretreatment unit, step (2) is performed in the PECVD parallel tube of the PECVD deposition unit, and step (3) is performed in the thermal annealing unit.
[0055] Example 3
[0056] This embodiment provides a method for preparing a boron emitter by depositing a BSG-boron source layer by PECVD, the method comprising the following steps:
[0057] (1) Using KOH solution to clean and texturize the silicon wafer to form a velvet surface on the surface of the silicon wafer;
[0058] (2) placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, wherein the deposition temperature is 250° C., the pressure is 3000 mTorr, the time is 8000 s, the power is 5000 W, the pulse switch ratio is 1 / 100, the power frequency is 40 kHz, the process gas includes 1 slm of SiH4, 0.1 slm of B2H6 and 1 slm of N2O, and the dilution gas is 6 slm of N2;
[0059] (3) subjecting the silicon wafer to a thermal annealing treatment at a temperature of 800° C., a time of 300 min, and a pressure of 1060 mbar, with a flow rate of 1.5 slm of N2 and 1.5 slm of O2 being introduced during the thermal annealing treatment;
[0060] (4) The BSG layer on the surface of the silicon wafer is removed using an HF solution with a volume fraction of 80%.
[0061] The device system used in the method provided in this embodiment includes a silicon wafer pretreatment unit, a PECVD deposition unit and a thermal annealing unit connected in sequence, and the PECVD deposition unit includes a PECVD parallel tube. Among them, step (1) is performed in the silicon wafer pretreatment unit, step (2) is performed in the PECVD parallel tube of the PECVD deposition unit, and step (3) is performed in the thermal annealing unit.
[0062] Example 4
[0063] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for shortening the deposition time in step (2) to 10 s, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0064] Example 5
[0065] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the deposition power in step (2) to 4000 W, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0066] Example 6
[0067] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the pulse switching ratio of the deposition in step (2) to 1 / 150, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0068] Example 7
[0069] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the deposition power frequency in step (2) to 30 kHz, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0070] Example 8
[0071] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the temperature of the thermal annealing treatment in step (3) to 600°C, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0072] Example 9
[0073] This embodiment provides a method for preparing a boron emitter by depositing a BSG-boron source layer by PECVD. Except for raising the temperature of the thermal annealing treatment in step (3) to 1040°C, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0074] Example 10
[0075] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for shortening the thermal annealing time in step (3) to 80 minutes, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0076] Embodiment 11
[0077] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the pressure of the thermal annealing treatment in step (3) to 800 mbar, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0078] Example 12
[0079] This embodiment provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for increasing the pressure of the thermal annealing treatment in step (3) to 1120 mbar, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0080] Comparative Example 1
[0081] This comparative example provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the deposition temperature in step (2) to 200°C, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0082] Comparative Example 2
[0083] This comparative example provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for increasing the deposition temperature in step (2) to 600°C, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0084] Comparative Example 3
[0085] This comparative example provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for reducing the deposition pressure in step (2) to 600 mTorr, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0086] Comparative Example 4
[0087] This comparative example provides a method for preparing a boron emitter by PECVD deposition of a BSG-boron source layer. Except for increasing the deposition pressure in step (2) to 3500 mTorr, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.
[0088] The performance parameters of the silicon wafers obtained in Examples 1-12 and Comparative Examples 1-4 are shown in Table 1 below.
[0089] Table 1
[0090]
[0091]
[0092] It can be seen from Table 1 that: Examples 1-12 utilize PECVD to deposit BSG and superimpose annealing to obtain ECV curves and film thicknesses close to those after secondary boron diffusion; compared with Example 1, Comparative Example 1 reduces the deposition temperature to 200°C, and process gases such as SiH4, B2H6 and N2O cannot be fully ionized, which easily causes abnormal film color and low surface concentration; Comparative Example 2 increases the deposition temperature to 600°C, and SiH4 and B2H6 decompose too quickly, which easily causes uneven film color at the furnace mouth and furnace tail, and most of the B2H6 will gather at the furnace mouth, resulting in a high concentration at the furnace mouth; Comparative Example 3 reduces the deposition pressure to 600mTorr, and the pumping speed at the furnace mouth is too fast, which easily causes the film color at the furnace mouth to be thin and the concentration to be low; Comparative Example 4 increases the deposition pressure to 3500mTorr, and the deposition at the furnace mouth is too much, which makes the film thickness at the furnace mouth thick, and then leads to a high concentration at the furnace mouth.
[0093] It can be seen that the present invention optimizes and improves the key condition parameters of the existing PECVD method for preparing a boron emitter by depositing a BSG-boron source layer, making it particularly suitable for depositing BSG on a large-diameter PECVD device for large-size series batteries, without significant wrap-around plating, strong process scalability, and not easy to form oxygen rings. It improves the uniformity and doping concentration of boron doping, reduces the difficulty of removing the surface BSG layer, improves the passivation effect, and at the same time simplifies the process flow, improves production efficiency, and is conducive to large-scale promotion and application.
[0094] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a boron emitter by depositing a BSG-boron source layer by PECVD, characterized in that: The method comprises sequentially performing silicon wafer pretreatment, PECVD deposition and thermal annealing; The PECVD deposition temperature is 250-500°C, the pressure is 800-3000mTorr, the time is 0.1-8000s, the power is 5000-30000W, the pulse switch ratio is 1 / 100-1 / 5, the power frequency is 40-200kHz, the process gas includes 0.1-1slm SiH4, 0.1-1slm B2H6 and 0.1-1slm N2O, and the dilution gas includes any one of 0.01-1slm Ar, 0.01-1slm H2 or 2-10slm N2 or a combination of at least two thereof; The method is suitable for depositing BSG on PECVD equipment with a tube diameter of 520 mm or 540 mm for 182 mm series or 210 mm series batteries.
2. The method according to claim 1, characterized in that The silicon wafer pretreatment includes: cleaning and texturing the silicon wafer to form a texturing surface on the surface of the silicon wafer; or cleaning and polishing the silicon wafer to form a polishing surface on the surface of the silicon wafer.
3. The method according to claim 1, characterized in that: The PECVD deposition comprises: placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition.
4. The method according to claim 1, characterized in that: The thermal annealing treatment is performed at a temperature of 800-1100° C., a time of 10-300 min, and a pressure of 10-1060 mbar; During the thermal annealing process, N2 and / or O2 are introduced, and the flow rate is 0.01-3slm; After the thermal annealing treatment, an HF solution is used to remove the BSG layer on the surface of the silicon wafer, and the volume fraction of the HF solution is 15%-80%.
5. The method according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) cleaning and texturing the silicon wafer to form a velvet surface on the surface of the silicon wafer; or cleaning and polishing the silicon wafer to form a polished surface on the surface of the silicon wafer; (2) placing a silicon wafer into a graphite boat, and sending the graphite boat into a furnace tube for PECVD deposition, wherein the deposition temperature is 250-500° C., the pressure is 800-3000 mTorr, the time is 0.1-8000 s, the power is 5000-30000 W, the pulse switch ratio is 1 / 100-1 / 5, the power frequency is 40-200 kHz, the process gas includes 0.1-1 slm SiH4, 0.1-1 slm B2H6 and 0.1-1 slm N2O, and the dilution gas includes any one of 0.01-1 slm Ar, 0.01-1 slm H2 or 2-10 slm N2 or a combination of at least two thereof; (3) subjecting the silicon wafer to thermal annealing treatment at a temperature of 800-1100° C., a time of 10-300 min, and a pressure of 10-1060 mbar, and introducing N2 and / or O2 during the thermal annealing treatment at a flow rate of 0.01-3 slm; (4) Using HF solution to remove the BSG layer on the surface of the silicon wafer, and the volume fraction of the HF solution is 15%-80%.
6. A silicon wafer, characterized in that: The surface of the silicon wafer is provided with a boron emitter made by the method according to any one of claims 1 to 5.
7. A device system used in the method according to any one of claims 1 to 5, characterized in that: It includes a silicon wafer pretreatment unit, a PECVD deposition unit and a thermal annealing unit which are connected in sequence.
8. The device system according to claim 7, characterized in that: The PECVD deposition unit includes a PECVD parallel tube.
Citation Information
Patent Citations
Boron-doped selective emitter TOPcon battery and preparation method thereof
CN116190470A
Boron emitter and preparation method thereof, and N-type crystalline silicon cell
CN116190495A
Preparation method of solar cell, solar cell and photovoltaic module
CN117199176A