Metal-based metal foil plate for power semiconductor and circuit etching process thereof
Through the metal-based metal foil plate process on the circuit layer of the IGBT module, the design of the stacked structure and etching pattern is used to solve the serious problem of side corrosion of the circuit layer, improve the production quality and heat dissipation effect, and enhance the current carrying capacity.
Patent Information
- Application Number
- CN202410114835.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-01-29
AI Technical Summary
When the copper thickness of the IGBT module circuit layer is ≥75 μm, the side corrosion is serious, affecting the circuit accuracy. The existing multiple etching methods cause the side corrosion to intensify and reduce the production quality of the circuit layer.
The metal base clad metal foil board process is adopted, which includes sequentially stacking a metal substrate, a resin composition dielectric layer and a circuit layer. The thickness of the copper foil of the circuit layer is 0.01~1.0mm. The first and second etches are formed by etching on both sides of the circuit layer. Patterns to penetrate each other to reduce the amount of side erosion, and set raised patterns on the metal substrate to enhance bonding strength.
It effectively reduces the amount of undercutting of the circuit layer, improves the production quality and heat dissipation effect of the IGBT module circuit, and enhances the current carrying capacity.
Smart Images

Figure CN117769117B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of circuit board production, and more specifically, to a metal-based metal-foil-clad board for power semiconductors and a circuit etching process thereof. Background Art
[0002] In recent years, power semiconductors have developed rapidly, and the density of power semiconductors has been continuously improved. High-power electronic inverters made of power semiconductors have been widely used. Insulated-gate bipolar transistor (IGBT) is a power semiconductor device widely used in energy storage converters, wind power converters, photovoltaic inverters and general-purpose converters. IGBT modules play an important role in the new energy electric vehicle industry. The main requirements of the substrate of the IGBT module are to ensure the current carrying capacity and stabilize the power supply.
[0003] The development trend of IGBT modules is to carry larger currents and be able to dissipate the large amount of heat generated in a timely manner. The copper foil thickness of the circuit layer of the IGBT module is getting thicker and thicker. The high current characteristics of the IGBT module make the copper thickness of the circuit layer of the IGBT module larger. The IGBT module often has an ultra-thick copper foil circuit of 4Oz to 10Oz. During the production process of the circuit layer of the IGBT module, when the copper thickness is ≥75μm (about 2Oz), the side etching of its conductive copper path will become very obvious. Specifically, for the circuit layer with a copper foil thickness greater than 4Oz, multiple etching methods are generally used for processing during etching, but the more times the etching is performed, the more serious the side etching of the circuit will be, and the greater the impact on the accuracy of the circuit of the IGBT module will be. Summary of the invention
[0004] The purpose of this application is to provide a metal-based metal foil plate for power semiconductors and its circuit etching process, which solves the technical problem of serious side etching of the circuit layer of the existing IGBT module and achieves the technical effect of improving the production quality of the circuit layer structure of the IGBT module.
[0005] The embodiment of the present application provides a metal-based metal-clad foil plate for power semiconductors. The metal-based metal-clad foil plate includes a metal substrate, a resin composition dielectric layer and a circuit layer stacked in sequence. The metal substrate is used for the heat dissipation structure of the metal-based metal-clad foil plate. The thermal conductivity of the resin composition dielectric layer is 0.3 to 30 W (m·°C). The circuit layer is used to fix the IGBT chip. The copper foil thickness of the circuit layer is 0.01 to 1.0 mm. A first etching pattern is provided on a side of the circuit layer close to the metal substrate, and a second etching pattern is provided on a side of the circuit layer away from the metal substrate. After the first etching pattern and the second etching pattern are processed separately, they penetrate each other to form a circuit pattern of the circuit layer.
[0006] In a possible implementation manner, the etching depth of the first etching pattern and the second etching pattern is 1 / 3 to 2 / 3 of the thickness of the copper foil of the circuit layer.
[0007] In another possible implementation, a side etching groove is retained on the sidewall of the etching groove of the first etching pattern.
[0008] In another possible implementation, a protruding pattern corresponding to the first etching pattern is provided on the metal substrate, the protruding pattern is embedded between the circuits of the first etching pattern, and the resin composition dielectric layer fills the gap between the protruding pattern and the first etching pattern.
[0009] In another possible implementation, the protruding pattern is formed by performing a rapid etching process on the surface of the metal substrate, and a smooth structure is formed at the top edge of the protruding structure of the protruding pattern by rapid etching.
[0010] In another possible implementation, the etching depth of the protruding pattern is 1 / 2 to 2 / 3 of the etching depth of the first etching pattern.
[0011] The embodiment of the present application also provides a circuit etching process for a metal-based metal-clad foil plate for power semiconductors, which is used to produce the above-mentioned metal-based metal-clad foil plate for power semiconductors. The process includes: fixing the circuit layer copper foil, and etching a first etching pattern on one side of the circuit layer copper foil; wherein the thickness of the circuit layer copper foil is 0.01 to 1.0 mm; stacking a metal substrate, a resin composition dielectric layer and a circuit layer copper foil in sequence and pressing them together; wherein the side where the first etching pattern of the circuit layer copper foil is located is bonded to the resin composition dielectric layer, and the thermal conductivity of the resin composition dielectric layer is 0.3 to 30 W (m·℃); etching a second etching pattern on the side of the circuit layer copper foil away from the metal substrate; wherein the first etching pattern and the second etching pattern penetrate each other to form a circuit pattern.
[0012] In another possible implementation, etching a first etching pattern on one side of the circuit layer copper foil includes: performing at least two rapid etchings to reduce the width of the etching area with reference to the first etching pattern; wherein the sidewalls of the etching grooves of the first etching pattern retain side etching grooves.
[0013] In another possible implementation, the method further includes: protruding a raised pattern on the surface of the metal substrate by etching on the metal substrate, the raised pattern corresponding to the first etching pattern; sequentially stacking the metal substrate, the resin composition dielectric layer and the circuit layer copper foil and laminating them, including: during lamination, the raised pattern is embedded between the circuits of the first etching pattern, and the resin composition dielectric layer fills the gap between the raised pattern and the first etching pattern.
[0014] In another possible implementation, the line width of the protruding pattern is reduced compared to the gap between the lines of the first etching pattern.
[0015] In another possible implementation manner, the method further includes: forming a rounded structure at a top edge of the protruding structure of the protruding pattern by rapid etching.
[0016] In another possible implementation, the metal substrate, the resin composition dielectric layer and the circuit layer copper foil are sequentially stacked and pressed under vacuum conditions.
[0017] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0018] The embodiment of the present application provides a metal-based metal-clad foil plate for power semiconductors, the metal-based metal-clad foil plate comprises a metal substrate, a resin composition dielectric layer and a circuit layer stacked in sequence, the metal substrate is used for the heat dissipation structure of the metal-based metal-clad foil plate, the thermal conductivity of the resin composition dielectric layer is 0.3-30W (m·℃), the circuit layer is used to fix the IGBT chip, the copper foil thickness of the circuit layer is 0.01-1.0mm, a first etching pattern is provided on the side of the circuit layer close to the metal substrate, and a second etching pattern is provided on the side of the circuit layer away from the metal substrate, and the first etching pattern and the second etching pattern are respectively processed and penetrate each other to form a circuit pattern of the circuit layer. The embodiment of the present application can improve the heat dissipation effect of the IGBT module through the metal substrate, and can effectively reduce the side etching amount of the circuit layer by etching the two sides of the circuit layer and bonding the circuit layer to the metal substrate, thereby improving the production effect of the circuit of the IGBT module. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0020] Figure 1 It is a structural schematic diagram of an existing IGBT module;
[0021] Figure 2 It is a structural schematic diagram of another existing IGBT module;
[0022] Figure 3 This is a schematic structural diagram of a metal-based metal foil plate for power semiconductors in an embodiment of the present application;
[0023] Figure 4 This is a schematic structural diagram of another metal-based metal foil-clad plate for power semiconductors in an embodiment of the present application;
[0024] Figure 5 for Figure 4 Schematic diagram of the local structure at A in FIG.
[0025] Figure 6 This is a schematic diagram of the production process of a metal-based metal-clad foil plate for power semiconductors in an embodiment of the present application;
[0026] Figure 7 A schematic diagram of the production process of another metal-based metal-clad foil plate for power semiconductors in an embodiment of the present application;
[0027] Figure 8 It is a schematic diagram of a process flow of etching a circuit of a metal-based metal foil plate for a power semiconductor in an embodiment of the present application;
[0028] In the figure, 1, metal base metal foil plate; 11, metal substrate; 111, protrusion pattern; 12, resin composition dielectric layer; 13, circuit layer; 13a, circuit layer copper foil; 131, first etching pattern; 131a, side etching groove; 132, second etching pattern; 133, circuit pattern; 21, substrate; 211, chip; 22, bottom plate; 221, bottom plate solder layer; 23, heat sink; 231, thermal grease. DETAILED DESCRIPTION
[0029] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0030] It should be noted that when a component or structure is referred to as being "fixed to" or "disposed on" another component or structure, it may be directly on the other component or structure or indirectly on the other component or structure. When a component or structure is referred to as being "connected to" another component or structure, it may be directly connected to the other component or structure or indirectly connected to the other component or structure.
[0031] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or a component or structure referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0033] Figure 1 FIG. 1 is a schematic diagram of the structure of an existing IGBT module. Figure 1 As shown, an existing IGBT module includes a substrate 21, a bottom plate 22 and a heat sink 23. A chip 211 is fixedly connected to the substrate 21. The chip 211 can be an IGBT chip. The substrate 21 is connected to the bottom plate 22 through a bottom plate solder layer 221. The bottom plate 22 is a shell structure of the IGBT module. The bottom plate 22 can also be connected to the heat sink 23 through thermal grease 231. The heat sink 23 can dissipate the heat conducted by the substrate 21 and the chip 211.
[0034] Figure 2 It is a structural diagram of another existing IGBT module, such as Figure 2 As shown, another existing IGBT module includes a substrate 21 and a heat sink 23. A chip 211 is fixedly connected to the substrate 21. The chip 211 can be an IGBT chip. The substrate 21 is connected to the heat sink 23 through a thermal grease 231. The heat sink 23 can dissipate the heat conducted by the substrate 21 and the chip 211.
[0035] like Figure 1 and Figure 2 As shown, the existing substrate 21 may include a conductive layer and an insulating plate, and the insulating plate may be made of glass fiber cloth, epoxy resin, polyimide or a ceramic substrate, etc. However, the heat dissipation effect of the substrate 21 made of the existing insulating plate is poor. For example, the thermal conductivity of the substrate 21 packaged by the ceramic copper clad substrate is insufficient, so that the IGBT module using the substrate 21 has a long heat conduction path from the chip to the base plate 22 and the heat sink 23, resulting in a large thermal resistance of the IGBT module when dissipating heat.
[0036] In addition, the high current characteristics of the IGBT module make the copper thickness of the circuit layer of the IGBT module relatively large, and the IGBT module often has ultra-thick copper foil circuits of 4Oz to 10Oz. For the circuit layer with a copper foil thickness greater than 4Oz, multiple etching methods are generally used for processing during etching. However, the more etching times, the more serious the side etching of the circuit will be, and the greater the impact on the accuracy of the circuit of the IGBT module will be.
[0037] Based on the above reasons, the embodiment of the present application provides a metal-based metal-clad foil plate for power semiconductors, the metal-based metal-clad foil plate includes a metal substrate, a resin composition dielectric layer and a circuit layer stacked in sequence, the metal substrate is used for the heat dissipation structure of the metal-based metal-clad foil plate, the thermal conductivity of the resin composition dielectric layer is 0.3-30W (m·℃), the circuit layer is used to fix the IGBT chip, the copper foil thickness of the circuit layer is 0.01-1.0mm, the side of the circuit layer close to the metal substrate is provided with a first etching pattern, the side of the circuit layer away from the metal substrate is provided with a second etching pattern, the first etching pattern and the second etching pattern are respectively processed and penetrate each other to form a circuit pattern of the circuit layer. The embodiment of the present application can improve the heat dissipation effect of the IGBT module through the metal substrate, and can effectively reduce the side etching amount of the circuit layer by etching the two sides of the circuit layer and bonding the circuit layer to the metal substrate, thereby improving the production effect of the circuit of the IGBT module.
[0038] In some scenarios, a metal-based metal foil-clad plate for power semiconductors according to an embodiment of the present application can be used to produce IGBT modules with high heat dissipation, and can reduce the amount of side corrosion of the circuit of the IGBT module.
[0039] The following is a detailed description of a metal-based metal foil-clad plate for power semiconductors and a circuit etching process thereof provided in an embodiment of the present application with reference to specific examples.
[0040] Figure 3 Schematic diagram of the structure of a metal-based metal foil plate for power semiconductors in an embodiment of the present application. Figure 3 As shown, the metal-based metal-clad foil plate 1 in the embodiment of the present application includes a metal substrate 11, a resin composition dielectric layer 12 and a circuit layer 13 stacked in sequence, the metal substrate 11 is used for the heat dissipation structure of the metal-based metal-clad foil plate 1, the thermal conductivity of the resin composition dielectric layer 12 is 0.3~30W(m·℃), the circuit layer 13 is used to fix the IGBT chip 131, the copper foil thickness of the circuit layer 13 is 0.01~1.0mm, and a first etching pattern 131 is provided on the side of the circuit layer 13 close to the metal substrate 11, and a second etching pattern 132 is provided on the side of the circuit layer 13 away from the metal substrate 11. After the first etching pattern 131 and the second etching pattern 132 are processed respectively, they penetrate each other to form a circuit pattern 133 of the circuit layer 13.
[0041] like Figure 3 As shown, structurally, the metal substrate 11 serves as a heat dissipation structure of the metal-based metal foil plate 1, which can conduct the metal-based metal foil plate 1 to dissipate heat. The thermal conductivity of the resin composition dielectric layer 12 is 0.3 to 30 W (m·℃). The circuit layer 13 is used to fix the IGBT chip 131, so that the resin composition dielectric layer 12 can efficiently conduct heat from the circuit layer 13 to the metal substrate 11.
[0042] Structurally, the copper foil thickness of the circuit layer 13 is 0.01 to 1.0 mm. A first etching pattern 131 is provided on the side of the circuit layer 13 close to the metal substrate 11, and a second etching pattern 132 is provided on the side of the circuit layer 13 away from the metal substrate 11. After the first etching pattern 131 and the second etching pattern 132 are processed separately, they penetrate each other to form a circuit pattern 133 of the circuit layer 13.
[0043] During use, when producing the circuit graphic 133 on the circuit layer 13, a first etching graphic 131 can be provided on the side of the circuit layer 13 close to the metal substrate 11, and a second etching graphic 132 can be provided on the side of the circuit layer 13 away from the metal substrate 11, and the first etching graphic 131 and the second etching graphic 132 are respectively processed and penetrate each other to form the circuit graphic 133 of the circuit layer 13, so that the circuit graphic 133 can be assembled by two separate etchings, thereby reducing the side etching amount of the circuit graphic 133 during production, improving the production quality of the circuit graphic 133, and ensuring the current carrying capacity of the circuit graphic 133.
[0044] The beneficial effect brought about by the above-mentioned implementation method is that after the first etching pattern and the second etching pattern are processed separately, they penetrate each other to form a circuit pattern of the circuit layer, so that the circuit pattern can be assembled by two separate etchings, thereby reducing the side etching amount of the circuit pattern during production, improving the production quality of the circuit pattern, and ensuring the current carrying capacity of the circuit pattern.
[0045] In some implementations, the etching depth of the first etching pattern 131 and the second etching pattern 132 is 1 / 3 to 2 / 3 of the thickness of the copper foil of the circuit layer 13 .
[0046] When in use, the etching depth of the first etching pattern 131 and the second etching pattern 132 is 1 / 3 to 2 / 3 of the copper foil thickness of the circuit layer 13, so that the etching depth of the first etching pattern 131 and the second etching pattern 132 will not be greater than 2 / 3 of the copper foil thickness of the circuit layer 13, so that the etching depth of the first etching pattern 131 and the second etching pattern 132 will not be too large, thereby avoiding excessive side etching during the production of the first etching pattern 131 and the second etching pattern 132.
[0047] Exemplarily, the etching depth of the first etching pattern 131 and the second etching pattern 132 is 1 / 2 of the thickness of the copper foil of the circuit layer 13 .
[0048] By way of example, the etching depths of the first etching pattern 131 and the second etching pattern 132 may be 1 / 3 and 2 / 3 of the thickness of the copper foil of the circuit layer 13 , respectively.
[0049] The beneficial effect brought by the above implementation method is that the etching depth of the first etching pattern and the second etching pattern will not be greater than 2 / 3 of the copper foil thickness of the circuit layer, which can avoid excessive side etching of the first etching pattern and the second etching pattern.
[0050] In some implementations, the sidewalls of the etching grooves of the first etching pattern 131 retain an undercut groove 131 a .
[0051] Figure 4 This is a schematic structural diagram of another metal-based metal foil plate for power semiconductors in an embodiment of the present application. Figure 5 for Figure 4 The local structure diagram at A in FIG. Figure 4 and Figure 5 As shown, structurally, the sidewall of the etching groove of the first etching pattern 131 retains a side etching groove 131a. Since the side etching groove 131a is bent laterally from the sidewall of the etching groove of the first etching pattern 131, the resin composition dielectric layer 12 can be embedded in the side etching groove 131a, which can improve the bonding strength between the side etching groove 131a and the resin composition dielectric layer 12, and can improve the bonding strength between the circuit layer 13 and the resin composition dielectric layer 12.
[0052] The beneficial effect brought by the above implementation method is that by embedding the resin composition dielectric layer into the undercut groove, the bonding force between the undercut groove and the resin composition dielectric layer can be improved, thereby improving the bonding force between the circuit layer and the resin composition dielectric layer.
[0053] In some implementations, Figure 6 This is a schematic diagram of the production process of a metal-based metal-clad foil plate for power semiconductors in an embodiment of the present application. Figure 7 Schematic diagram of the production process of another metal-based metal foil plate for power semiconductors in the embodiment of the present application. Figure 6 and Figure 7 As shown, a protruding pattern 111 corresponding to the first etching pattern 131 is provided on the metal substrate 11 , the protruding pattern 111 is embedded between the lines of the first etching pattern 131 , and the resin composition dielectric layer 12 fills the gap between the protruding pattern 111 and the first etching pattern 131 .
[0054] like Figure 6 and Figure 7 As shown, structurally, a protruding pattern 111 corresponding to the first etching pattern 131 is provided on the metal substrate 11, and the protruding pattern 111 is embedded between the circuits of the first etching pattern 131, so that the protruding pattern 111 can increase the bonding force between the metal substrate 11 and the circuit layer 13.
[0055] Structurally, the resin composition dielectric layer 12 fills the gap between the protruding pattern 111 and the first etching pattern 131. Since the protruding pattern 111 is embedded between the lines of the first etching pattern 131, the thickness between the protruding pattern 111 and the lines of the first etching pattern 131 is reduced, thereby improving the thermal conductivity between the metal substrate 11 and the circuit layer 13.
[0056] Structurally, the resin composition dielectric layer 12 fills the gap between the protruding pattern 111 and the first etching pattern 131. Since the protruding pattern 111 is embedded between the circuits of the first etching pattern 131, the contact area between the metal substrate 11 and the circuit layer 13 is increased, thereby improving the thermal conductivity between the metal substrate 11 and the circuit layer 13.
[0057] The beneficial effect brought about by the above-mentioned implementation method is that the protruding pattern is embedded between the circuits of the first etching pattern, and the resin composition dielectric layer fills the gap between the protruding pattern and the first etching pattern, so that the thickness of the resin composition dielectric layer between the metal substrate and the circuit layer is reduced, and the contact area between the metal substrate and the circuit layer is increased. In addition, the protruding pattern is embedded between the circuits of the first etching pattern, so that the protruding pattern can increase the bonding force between the metal substrate and the circuit layer.
[0058] In some implementations, the protruding pattern 111 is formed by performing a rapid etching process on the surface of the metal substrate 11 , and a smooth structure is formed at the top edge of the protruding structure of the protruding pattern 111 by rapid etching.
[0059] like Figure 7 As shown, structurally, the protruding pattern 111 is formed by rapid etching on the surface of the metal substrate 11, so that the protruding pattern 111 can be rapidly formed by coating a film, exposing, etching and cleaning, and the protruding pattern can be rapidly processed.
[0060] Structurally, a smooth structure is formed at the top edge of the protruding structure of the protruding pattern 111 by rapid etching, which can facilitate the resin composition dielectric layer to smoothly fill the gap between the protruding pattern and the first etching pattern.
[0061] The beneficial effect brought by the above implementation method is that by quickly etching the top edge of the raised structure of the raised pattern to form a smooth structure, the resin composition dielectric layer can be promoted to smoothly fill the gap between the raised pattern and the first etched pattern, thereby improving the matching effect between the raised pattern and the first etched pattern.
[0062] In some implementations, the etching depth of the protrusion pattern 111 is ½ to 2 / 3 of the etching depth of the first etching pattern 131 .
[0063] like Figure 7As shown, illustratively, in structure, the etching depth of the protruding pattern 111 is 1 / 2 to 2 / 3 of the etching depth of the first etching pattern 131, and a sufficient gap can be left between the protruding pattern 111 and the first etching pattern 131, so that the gap between the protruding pattern and the first etching pattern can be fully filled by the resin composition dielectric layer.
[0064] The beneficial effect brought by the above implementation manner is that a sufficient gap is left between the protruding pattern and the first etching pattern, and the gap between the protruding pattern and the first etching pattern can be fully filled by the resin composition dielectric layer.
[0065] The embodiment of the present application also provides a circuit etching process for a metal-based metal-clad foil plate for power semiconductors, which is used to produce any of the metal-based metal-clad foil plates for power semiconductors as described above. The process includes S110 to S130, and S110 to S130 are described in detail below.
[0066] S110, fix the circuit layer copper foil 13a, and etch a first etching pattern 131 on one side of the circuit layer copper foil 13a. The thickness of the circuit layer copper foil 13a is 0.01-1.0 mm.
[0067] During production, the first etching pattern 131 is etched on one side of the circuit layer copper foil 13a, thereby reducing the side etching amount of the circuit layer copper foil 13a compared to directly etching through the circuit layer copper foil 13a.
[0068] In terms of structure, the thickness of the circuit layer copper foil 13a is 0.01-1.0 mm, which facilitates etching of the thicker circuit layer copper foil 13a and ensures the current carrying capacity of the circuit layer copper foil 13a.
[0069] S120, stacking the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a in sequence and pressing them together. The side where the first etching pattern 131 of the circuit layer copper foil 13a is located is bonded to the resin composition dielectric layer 12, and the thermal conductivity of the resin composition dielectric layer 12 is 0.3 to 30 W (m·°C).
[0070] Structurally, the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a are stacked in sequence and pressed together, so that the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a can form the basic structure of the metal-based metal foil-clad board 1 after pressing together.
[0071] Structurally, the side of the circuit layer copper foil 13a where the first etching pattern 131 is located is bonded to the resin composition dielectric layer 12, and then the side of the circuit layer copper foil 13a away from the first etching pattern 131 can be etched to complete the complete circuit layer pattern.
[0072] The thermal conductivity of the resin composition dielectric layer 12 is 0.3-30 W (m·° C.), and the resin composition dielectric layer 12 can ensure the thermal conductivity between the metal substrate 11 and the circuit layer copper foil 13 a.
[0073] S130, etching a second etching pattern 132 on the side of the circuit layer copper foil 13a away from the metal substrate 11. The first etching pattern 131 and the second etching pattern 132 penetrate each other to form a circuit pattern 133.
[0074] During production, the second etching pattern 132 is etched on the side of the circuit layer copper foil 13a away from the first etching pattern 131, that is, the second etching pattern 132 is etched on the side of the circuit layer copper foil 13a away from the metal substrate 11, so that the first etching pattern 131 and the second etching pattern 132 penetrate each other to form a circuit pattern 133, thereby avoiding the problem of excessive side etching when producing the circuit pattern 133.
[0075] The beneficial effect brought by the above implementation method is that, by etching the circuit pattern twice, the problem of excessive side etching during the production of the circuit pattern is avoided, and the circuit production quality of the metal-based metal foil-clad board is improved.
[0076] In some implementations, the etching process of the first etching pattern 131 on one side of the circuit layer copper foil 13a includes: performing at least two rapid etchings respectively to reduce the width of the etching area with reference to the first etching pattern 131. The sidewall of the etching groove of the first etching pattern 131 retains a side etching groove 131a.
[0077] like Figures 4 to 6 As shown, structurally, when etching the first etching pattern 131, at least two rapid etchings can be performed respectively by using the first etching pattern 131 as a reference to reduce the width of the etching area, thereby effectively avoiding the phenomenon that the line width of the first etching pattern 131 does not meet the standard due to side etching, thereby ensuring the current carrying capacity of the first etching pattern 131.
[0078] Structurally, after the first etching pattern 131 is produced, a side etching groove 131a can be retained on the side wall of the etching groove of the first etching pattern 131. By retaining the side etching groove 131a, the resin composition dielectric layer 12 can be filled into the first etching pattern 131 and the side etching groove 131a, which can improve the bonding force between the first etching pattern 131 and the resin composition dielectric layer 12.
[0079] The beneficial effect brought by the above implementation method is that the resin composition dielectric layer can be filled into the first etching pattern and the side etching groove, which can improve the bonding force between the first etching pattern and the resin composition dielectric layer and avoid delamination and cracking of the metal-based metal foil-clad plate.
[0080] In some implementations, the process further includes: protruding a protruding pattern 111 disposed on the surface of the metal substrate 11 by etching the metal substrate 11 , the protruding pattern 111 and the first etching pattern 131 corresponding to the protruding pattern 111 .
[0081] The protruding pattern 111 disposed on the surface of the metal substrate 11 is protruded by etching on the metal substrate 11 , and the required pattern of the protruding pattern 111 can be conveniently processed by the etching process.
[0082] Structurally, the protruding pattern 111 corresponds to the first etching pattern 131 , so that the protruding pattern 111 can cooperate with each other to improve the bonding force between the first etching pattern 131 and the protruding pattern 111 .
[0083] In some implementations, the metal substrate 11, the resin composition dielectric layer 12, and the circuit layer copper foil 13a are sequentially stacked and pressed, including: during pressing, the raised pattern 111 is embedded between the lines of the first etched pattern 131, and the resin composition dielectric layer 12 fills the gap between the raised pattern 111 and the first etched pattern 131.
[0084] During production, after the protruding pattern 111 and the first etching pattern 131 are aligned with each other, the protruding pattern 111 can be embedded between the lines of the first etching pattern 131 during pressing, and the resin composition dielectric layer 12 fills the gap between the protruding pattern 111 and the first etching pattern 131, thereby improving the heat transfer effect between the protruding pattern 111 and the first etching pattern 131, and improving the bonding strength between the first etching pattern and the resin composition dielectric layer, thereby avoiding delamination and cracking of the metal-based metal foil-clad plate.
[0085] The beneficial effect brought by the above implementation method is that the protruding pattern is processed by etching on the metal substrate, and the heat transfer effect of the protruding pattern and the first etching pattern is improved by the protruding pattern, and the bonding force between the first etching pattern and the resin composition dielectric layer is improved, thereby avoiding delamination and cracking of the metal-based metal foil-clad plate.
[0086] In some implementations, the line width of the protruding pattern 111 is reduced compared to the gap between the lines of the first etching pattern 131 .
[0087] When etching the raised pattern 111, the line width of the raised pattern 111 can be reduced compared to the gap between the lines of the first etching pattern 131, so that the raised pattern 111 can be smoothly matched between the lines of the first etching pattern 131, thereby improving the production quality of the metal-based metal foil-clad plate 1.
[0088] The beneficial effect brought by the above implementation method is that the protruding pattern is reduced in size so that the protruding pattern can be smoothly matched between the circuits of the first etching pattern, thereby improving the production quality of the metal-based metal-clad foil plate.
[0089] In some implementations, the above process further includes: forming a rounded structure at the top edge of the protruding structure of the protruding pattern 111 by rapid etching.
[0090] When in use, a smooth structure can be formed by rapid etching at the top edge of the raised structure of the raised pattern 111, so that the resin composition dielectric layer can smoothly fill the gap between the raised pattern and the first etched pattern through the smooth structure of the raised structure of the raised pattern 111, and the smooth structure of the raised structure of the raised pattern 111 will not block the resin composition dielectric layer.
[0091] The beneficial effect brought by the above implementation method is that by quickly etching the top edge of the raised structure of the raised pattern to form a smooth structure, the resin composition dielectric layer can be promoted to smoothly fill the gap between the raised pattern and the first etched pattern, thereby improving the matching effect between the raised pattern and the first etched pattern.
[0092] In some implementations, the metal substrate 11 , the resin composition dielectric layer 12 , and the circuit layer copper foil 13 a are sequentially stacked and pressed under vacuum conditions.
[0093] During production, the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a can be stacked and pressed under vacuum conditions to discharge the internal gas of the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a during pressing, and can ensure that the resin composition dielectric layer 12 fills the gap between the protruding pattern 111 and the first etching pattern 131. The gas in the gap is effectively discharged, further improving the tightness of the bonding between the metal substrate 11, the resin composition dielectric layer 12 and the circuit layer copper foil 13a.
[0094] The beneficial effect brought by the above implementation method is that when the resin composition dielectric layer fills the gap between the protruding pattern and the first etching pattern, the gas in the gap is effectively discharged, further improving the tightness of the combination of the metal substrate, the resin composition dielectric layer and the circuit layer copper foil.
[0095] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A circuit etching process for a metal-based metal foil plate for power semiconductors, characterized in that: include: The circuit layer copper foil (13a) is fixed, and a first etching pattern (131) is etched on one side of the circuit layer copper foil (13a); wherein the thickness of the circuit layer copper foil (13a) is 0.01-1.0 mm; Etching a first etching pattern (131) on one side of a circuit layer copper foil (13a), comprising: Using the first etching pattern (131) as a reference, the width of the etching area is reduced and rapid etching is performed at least twice; wherein the sidewalls of the etching grooves of the first etching pattern (131) retain side etching grooves (131a); A protruding pattern (111) protrudes from the surface of the metal substrate (11) by etching the metal substrate (11), wherein the protruding pattern (111) corresponds to the first etching pattern (131); A metal substrate (11), a resin composition dielectric layer (12), and a circuit layer copper foil (13a) are sequentially stacked and pressed together; wherein, during the pressing, the raised pattern (111) is embedded between the lines of the first etching pattern (131), and the resin composition dielectric layer (12) fills the gap between the raised pattern (111) and the first etching pattern (131), and the thermal conductivity of the resin composition dielectric layer (12) is 0.3-30 W (m·°C); A second etching pattern (132) is etched on a side of the circuit layer copper foil (13a) away from the metal substrate (11); wherein the first etching pattern (131) and the second etching pattern (132) penetrate each other to form a circuit pattern (133).
2. The circuit etching process according to claim 1, characterized in that: The line width of the protruding pattern (111) is reduced compared to the gap between the lines of the first etching pattern (131).
3. A metal-based metal-foil-clad plate for power semiconductors, the metal-based metal-foil-clad plate being prepared by the circuit etching process according to any one of claims 1 to 2, characterized in that: The metal-based metal foil-clad plate (1) comprises a metal substrate (11), a resin composition dielectric layer (12) and a circuit layer (13) which are stacked in sequence. The metal substrate (11) is used for the heat dissipation structure of the metal-based metal foil-clad plate (1). The thermal conductivity of the resin composition dielectric layer (12) is 0.3-30 W (m·°C). The circuit layer (13) is used for fixing an IGBT chip. The copper foil thickness of the circuit layer (13) is 0.01-1.0 mm. A first etching pattern (131) is provided on a side of the circuit layer (13) close to the metal substrate (11). A second etching pattern (132) is provided on a side of the circuit layer (13) away from the metal substrate (11). After the first etching pattern (131) and the second etching pattern (132) are processed respectively, they penetrate each other to form a circuit pattern (133) of the circuit layer (13). A protruding pattern (111) corresponding to a first etching pattern (131) is provided on the metal substrate (11); the protruding pattern (111) is embedded between the lines of the first etching pattern (131); and a resin composition dielectric layer (12) fills the gap between the protruding pattern (111) and the first etching pattern (131); the protruding pattern (111) is formed by performing a rapid etching process on the surface of the metal substrate (11); and a smooth structure is formed at the top edge of the protruding structure of the protruding pattern (111) by rapid etching.
4. The metal-based metal-clad foil plate for power semiconductor according to claim 3, characterized in that: The etching depth of the first etching pattern (131) and the second etching pattern (132) is 1 / 3 to 2 / 3 of the thickness of the copper foil of the circuit layer (13).
5. The metal-based metal-clad foil plate for power semiconductor according to claim 3, characterized in that: The etching depth of the protruding pattern (111) is 1 / 2 to 2 / 3 of the etching depth of the first etching pattern (131).
Citation Information
Patent Citations
Super-thick copper diagram manufacturing method and printed circuit board (PCB) provided with super-thick copper diagram
CN103188875A
A circuit board and a manufacturing method thereof
CN104219867A
Flexible printed circuit thick copper etching prefabricated plate and manufacturing process thereof
CN110740587A
Manufacturing method of thick copper circuit board
CN117377221A
Manufacture of thick copper circuit board
JP1996222838A