Preparation method and application of activated coke-based solid waste resource modification catalyst
By mixing active coke with waste polypropylene plastics to prepare active coke-based solid waste resource modification catalysts, the problems of active coke structural instability and polypropylene plastic resource treatment are solved, catalytic efficiency and structural stability are improved, and the catalytic stability is reduced. Preparation cost realizes efficient treatment of coking wastewater and resource recycling.
Patent Information
- Application Number
- CN202311780585.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-12-22
AI Technical Summary
In the prior art, the structure of active coke in coking wastewater treatment is not stable enough, the catalytic effect is limited, and the resource treatment of polypropylene plastics is urgent, and the existing catalyst preparation cost is high, making it difficult to meet the energy-saving and carbon reduction needs.
Mix active coke with waste polypropylene plastic for grinding, cleaning, drying, metal loading and pyrolysis treatment, and prepare an active coke-based solid waste resource modification catalyst for ozone catalytic oxidation treatment to improve catalytic efficiency and Structural stability and reduce preparation costs.
It improves the catalytic activity and efficiency of the catalyst, extends the use cycle, reduces the preparation cost, realizes the resource treatment of polypropylene plastic, improves the utilization rate and oxidation performance of ozone, and meets the requirements of green pollution reduction and carbon reduction.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, and in particular to a preparation method and application of an activated coke-based solid waste resource modification catalyst. Background Art
[0002] Ozone oxidation technology is widely used in the treatment of high-concentration COD wastewater in chemical industries such as coking wastewater, papermaking wastewater, and pharmaceutical wastewater due to its simple operating conditions, good treatment effect, and short treatment cycle. After the introduction of ozone catalytic oxidation catalysts, the oxidation potential of ozone is significantly improved, and the generated can reduce the reaction activation energy or change the reaction process, inducing ozone decomposition to produce various free radicals with higher activity and lower selectivity than ozone, such as hydroxyl radicals, which can effectively improve the removal rate of large molecules and the mineralization rate of small molecules.
[0003] There are three types of commonly used ozone oxidation catalysts, mainly ceramsite, aluminum oxide and other carrier materials with high mechanical strength; manganese dioxide, zinc oxide, titanium dioxide and other highly active metal oxides; activated carbon, zeolite, activated coke and other porous materials with excellent adsorption properties. Among them, activated coke has both microporous and mesoporous structures, with a specific surface area of about 600~1000 m 2 / g, fast adsorption rate, strong selective adsorption ability, high adsorption capacity and low price. Relevant studies have shown that the pore size distribution of activated coke is highly compatible with the molecular diameter of refractory organic matter in the biochemical tail water of coking wastewater, and it has broad application prospects in the treatment of coking wastewater. However, compared with other catalytic materials, activated coke also has the limitations of unstable structure and limited catalytic effect.
[0004] In recent years, plastic products have been used more and more frequently. For example, polypropylene plastic, which can withstand high temperatures of 100°C, is not only used in food packaging, household items, automobiles, optical fibers, etc., but is also an important raw material for making disposable protective clothing and disposable masks. With the development of related industries, waste polypropylene plastic has become one of the largest solid waste polymer materials in recent years, and the demand for resource processing of polypropylene plastic has become more urgent.
[0005] In view of the above technical background, the present invention proposes a preparation method and application of an activated coke-based solid waste resource modification catalyst, in which activated coke is mixed with resource-recyclable polyethylene plastic for modification to form a new ozone catalyst for application in catalytic oxidation treatment of coking wastewater, thereby achieving improved removal efficiency, reduced preparation cost, and resource utilization of solid waste materials, thereby meeting the current transformation needs of energy-saving and carbon-reduction treatment of coking wastewater. Summary of the invention
[0006] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, which is characterized by comprising the following steps: 1) grinding and screening activated coke and solid waste materials; 2) soaking, cleaning, and drying the screened materials; 3) impregnating the dried materials with metal loads; and 4) calcining the mixture to obtain an activated coke carrier resource modification catalyst.
[0007] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, characterized in that activated coke and fruit shells, coconut shells, polyvinyl chloride plastics, polypropylene plastics, etc. are ground and then sieved through a 100-mesh sieve. Preferably, the solid waste material is waste polypropylene plastic, and the mass ratio of activated coke to polypropylene plastic is preferably 55%-80%:20%-45%.
[0008] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, characterized in that the activated coke and polypropylene plastic are sieved and then respectively removed from impurities by 1 mol / L and 0.1 mol / L nitric acid, and then respectively soaked and washed in deionized water for 30 to 120 min after acid washing, and the supernatant is discarded and then washed repeatedly for 2 to 3 times until there are no obvious impurities and the pH is near neutral. Preferably, the washing can be performed under the assistance of ultrasound for 30 to 60 min.
[0009] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, which is characterized in that the cleaned activated coke and polypropylene plastic are placed in a vacuum drying oven at 60-120°C for drying, preferably in a vacuum drying oven at 80-100°C for drying, and are isolated from air and cooled in a drying dish.
[0010] The present invention provides a preparation method and application of an active coke-based solid waste resource modification catalyst, characterized in that the mixture after washing and drying is impregnated into a metal nitrate solution of a certain concentration, wherein the metal nitrate solution is one or more of manganese, cerium, iron, nickel, and cobalt nitrate solutions, and the metal active component loading mass fraction is 2% to 15%. Preferably, the impregnation solution is a mixture of iron nitrate, cobalt nitrate, and nickel nitrate in proportion, and the mass fraction ratio is approximately iron: cobalt: nickel = 45% to 55%: 25% to 30%: 20% to 25%. The impregnation time is 24 to 96 hours, and preferably, the impregnation time can be 60 to 72 hours.
[0011] The invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, which is characterized in that a certain concentration of adhesive is added to a metal salt solution to improve the mechanical strength and structural stability of the activated coke and waste polypropylene plastic modification catalyst.
[0012] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, characterized in that the impregnated material is pyrolyzed in a nitrogen-protected tubular furnace at 400-900°C for 2-6 hours to obtain an activated coke carrier resource modification catalyst. The pyrolysis treatment temperature is preferably 700-900°C, the heating rate is 10°C / min, and the reaction time is preferably 2-4 hours.
[0013] The present invention provides a preparation method and application of an activated coke-based solid waste resource-based modified catalyst, which is characterized in that the resource-based modified catalyst can be applied to the ozone catalytic oxidation treatment of coking wastewater and biochemical sewage with a high COD concentration, and the modified material has higher catalytic activity and catalytic efficiency and stronger structural stability, while achieving resource-based treatment of waste polypropylene plastics and reducing the preparation cost of the catalyst.
[0014] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, characterized in that the ratio of the oxidant, i.e., ozone, to COD is about 1-2.5:1, and the catalyst dosage is about 20%-30%.
[0015] Based on the above invention content, the present invention has the beneficial effects of:
[0016] The present invention provides an activated coke-based solid waste resource modification catalyst, which has obvious advantages in improving catalytic efficiency and promoting the generation of hydroxyl radicals. The loaded active metal components on the catalyst surface can effectively increase the generation of hydroxyl radicals, while achieving the two major purposes of improving ozone utilization and oxidizability, thereby improving the overall oxidation performance and oxidation efficiency of ozone. Activated coke itself has a relatively good specific surface area, which can promote more metal actives to be loaded on the outer surface of the material, increase the contact area between the metal actives and ozone and pollutants, and enhance the ozone catalytic oxidation effect.
[0017] The present invention provides an activated coke-based solid waste resource modification catalyst, and the selection advantage of the activated coke carrier is obvious. Compared with ordinary silicon-aluminum-based catalysts, the activated coke carrier used in the present invention has better adsorption performance, and the pore size is more matched with the molecules in the coking wastewater, which can effectively improve the fouling of the catalyst pores by anions and cations in the coking wastewater. Compared with adsorption materials such as activated carbon with better adsorption performance, the present invention is low in cost. Due to the doping of a certain proportion of waste polypropylene plastics, on the basis of further reducing the cost of catalyst preparation, it provides a new idea for the resource treatment of waste polypropylene plastics that have been widely used in recent years, which meets the development needs of green pollution reduction and carbon reduction, and resource recycling.
[0018] The present invention provides an activated coke-based solid waste resource modification catalyst, which has obvious advantages in reducing the cost of catalyst preparation. The loaded metal active material is relatively tightly loaded on the outer surface of the material with the assistance of the binder, which effectively increases the mechanical strength of the catalyst and enhances the stability of the catalyst; it effectively prolongs the service life of the catalyst, which is conducive to the long-term and stable function of the catalyst, and reduces the trouble of replacing the catalyst and the economic cost caused by it. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention provides a comparison of the effects of different solid waste material resource-modified catalysts based on activated coke carriers on treating oxalic acid solutions.
[0020] Figure 2 The present invention provides an experimental effect of reuse of a modified catalyst based on the resource recovery of activated coke carrier. Implementation
[0021] The present invention provides a preparation method and application of an activated coke-based solid waste resource modification catalyst, wherein the resource modification catalyst has higher catalytic activity and catalytic efficiency than activated coke, and the binder improves the structural stability of the catalyst, prolongs the catalyst service life, realizes the resource treatment of solid waste materials, and reduces the preparation cost of the catalyst. The specific implementation method is as follows.
[0022] A preparation method and application of an activated coke-based solid waste resource modification catalyst, characterized in that the carrier material is a mixture of activated coke and resource-recyclable solid waste materials, such as fruit shells, coconut shells, polyethylene plastics, polyvinyl chloride plastics, polypropylene plastics, etc. Preferably, the solid waste material is waste polypropylene plastic, and the mass ratio of activated coke to polypropylene plastic is preferably 55%~80%:20%~45%. The specific operation steps for preparing the activated coke-based solid waste resource modification catalyst are as follows: 1) the activated coke and polypropylene plastic are mixed and crushed, and after screening, they are washed with high and low concentration nitric acid to remove impurities, and then washed with deionized water until the pH is near neutral; 2) the washed mixture is dried in a vacuum drying oven and cooled in a drying dish in an air-tight manner; 3) the dried mixture is placed in one or more nitrate solutions, and the metal active material loading treatment is completed with the assistance of a binder; preferably, the mass fraction ratio is approximately iron: cobalt: nickel = 45%~55%: 25%~30%: 20%~25%, and the immersion time can be 60~72 h; 4) the loaded material is placed in a nitrogen-protected tubular furnace for pyrolysis treatment to obtain an activated activated coke-based solid waste resource modification catalyst.
[0023] The present invention will be further described below in conjunction with the embodiments.
[0024] Example 1
[0025] The present invention provides a method for preparing an activated coke-based solid waste resource modification catalyst and its application, and screens the application effect of solid waste materials that can be recycled. The resource-based solid waste materials are selected from fruit shells, polyvinyl chloride plastics (Polyvinyl chloride, PVC), and polypropylene plastics (Polypropylene, PP), and are subjected to catalyst modification treatment with activated coke as a carrier under the same preparation conditions. The target pollutant described in the experiment is oxalic acid, which is a type of carboxylic acid and is often used as a target pollutant for judging the removal effect of catalysts. A 50 mg / L oxalic acid solution was treated with a catalyst prepared from 100 mg / L of different resource materials, maintaining consistent conditions, controlling the same temperature and pH, introducing 5 mg / min of ozone, and taking samples for detection at different times of the reaction. The removal effect is shown in the attached figure. Figure 1 As shown. Ozone alone can remove 76% of oxalic acid, "nutshell + ozone" and "PVC + ozone" have similar effects, and can remove 91% and 94% of oxalic acid after 60 minutes of reaction. "PP + ozone" has the best effect, and the removal rate of each sampling point is high, and 98% of oxalic acid can be removed in the end. This application example shows that the catalytic oxidation effect of the resource-based modified catalyst based on the activated coke carrier described in the present invention is good, and polypropylene plastic is feasible as a preferred resource material.
[0026] Example 2
[0027] A comparative application analysis was conducted on the biochemical sewage of a certain factory's coking wastewater. The basic experimental conditions were that the pH was about 7 and the temperature was about 28°C at room temperature. The application of ordinary silicon-aluminum-based catalysts can reduce the influent COD from 100 mg / L to about 53.4 mg / L, and the removal rate is about 46.6%. At this time, the catalyst dosage is about 26.7%, and the ozone concentration is 150 mg / L. The same sewage was treated with this catalyst, the catalyst usage was 25%, and the ozone concentration was 100 mg / L, which can achieve a removal rate of 57.7%, and the effluent concentration is as low as 42.3 mg / L. The two catalysts have limited removal effects on ammonia nitrogen, and have a certain effect on COD removal. The COD removal rate of the modified catalyst based on the resource recovery of activated coke carrier provided by the present invention is effectively improved.
[0028] Example 3
[0029] To evaluate the excellence of catalytic materials, it is also necessary to consider the reusability of the materials. This experiment conducted 5 repeated treatment tests on actual coking wastewater. The experimental water was the biochemical-coagulation effluent of a coking plant. The experimental results are as follows: Figure 2 As shown. Figure 2It can be seen that after the test, the catalyst can maintain a good ozone catalytic oxidation treatment effect when used repeatedly for 5 times. The COD concentration of the effluent from the 5 experiments is not much different, which can ensure that the COD of the biochemical-coagulation effluent quality of the coking wastewater is stable and meets the standard.
[0030] As mentioned above, although the typical embodiment designed by this invention was demonstrated, this invention is not limited to the said embodiment, Various corrections and changes can be implemented within the scope of a claim.
Claims
1. A method for preparing an activated coke-based solid waste resource modification catalyst, characterized in that: The resource-based modified catalyst is prepared from a carrier material and a metal active substance, wherein the carrier material is a mixture of activated coke and a resource-based solid waste material, wherein the solid waste material is waste polypropylene plastic, and the mass ratio of activated coke to waste polypropylene plastic is 55%-80%:20%-45%. The specific operation steps for preparing the activated coke-based solid waste resource-based modified catalyst are as follows: 1) The activated coke and polypropylene plastic are mixed and crushed, sieved, and washed with high and low concentration nitric acid to remove impurities, and then washed with deionized water until the pH is neutral; 2) The washed mixture is placed in a vacuum drying oven at 80-100°C for drying and then cooled in a drying dish in an airtight manner; 3) The dried mixture is placed in a nitrate solution, wherein the nitrate solution is a nitrate solution of iron, nickel and cobalt; the metal active material loading treatment is completed with the assistance of a binder; the mass fraction ratio of iron: cobalt: nickel is 45%~55%: 25%~30%: 20%~25%, and the immersion time is 60~72 h; 4) The impregnated material was pyrolyzed in a nitrogen-protected tubular furnace at 700-900°C with a heating rate of 10°C / min and a reaction time of 2-4 h to obtain an activated activated coke-based solid waste resource modification catalyst.
2. The method for preparing the activated coke-based solid waste resource modification catalyst according to claim 1, characterized in that: The mixture is ground and passed through a 100-mesh sieve. The sieved material is washed with 1 mol / L and 0.1 mol / L nitric acid to remove impurities. After acid washing, it is soaked in deionized water for 30 to 120 min. After discarding the supernatant, the washing is repeated 2 to 3 times until there are no obvious impurities and the pH is neutral.
3. The method for preparing the activated coke-based solid waste resource modification catalyst according to claim 1, characterized in that: A binder is added to the metal salt solution to assist in loading the metal active substance.
4. The catalyst obtained by the preparation method of the activated coke-based solid waste resource modification catalyst according to claim 1 is used for sewage treatment application research of oxalic acid solution and coking wastewater.