A Failure Analysis Method for Packaged Chip

Through the method of chemical solution heating to open the cap and epoxy glass carrier tape bonding, the technical problem of being unable to accurately determine the problem in the failure analysis of packaged chips has been solved, and more efficient detection and lower-cost production have been achieved.

CN117783832BActive Publication Date: 2024-10-01SHENZHEN EEVISION SEMICON TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410013517.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-10-01
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

The existing technology cannot accurately determine whether the failure of a packaged chip is due to problems caused by the chip itself or the packaging process, resulting in long detection time, high cost and waste of raw materials.

Method used

The chip is encapsulated using chemical solution to heat and open the cap, and a preset epoxy glass carrier tape is used for gold ball bonding and UV glue encapsulation. The type of chip failure is determined through a specific test platform to avoid damage to the chip.

Benefits of technology

It achieves more accurate and comprehensive failure analysis, reduces the duplication of comparative experimental groups and the waste of qualified chips, improves detection efficiency, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117783832B_ABST
    Figure CN117783832B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for failure analysis of packaged chips, including providing chemical solution and heating it, immersing the packaged chip to be analyzed in the chemical solution, completing the uncapping process of the packaged chip; selecting a preset epoxy glass carrier, loading the uncapped packaged chip onto the carrier, bonding the gold ball of the packaged chip; encapsulating and curing the bonded packaged chip; using a product testing platform adapted to the glass carrier, performing chip testing, and judging the failure type of the chip according to the test results. Through the non-destructive uncapping process, the damage to the chip function is avoided, so that more accurate and comprehensive analysis data can be obtained; bonding is then performed to simulate the packaged chip, so that the failure type of the problem chip is detected in a targeted manner according to the test results, reducing the repetition of the comparison experimental group and the waste of qualified chips, improving the detection efficiency, and being conducive to saving production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chip detection, and in particular to a failure analysis method for a packaged chip. Background Art

[0002] Flip-chip packaging is a method of mounting the chip on a wafer, then flipping it over and mounting it on a carrier tape using conductive glue or ultrasonic welding. For the specific structure, see the attached Figure 1 In the process of flip-chip packaging, since the chip is mounted on the carrier tape upside down, and a glue layer and gold balls are set on the contact surface between the chip and the carrier tape, it is difficult to determine whether the problem lies with the chip itself or in the packaging process in the event of product failure.

[0003] In the prior art, when analyzing failed packaged chips, since packaged products are usually multiple chips integrated together, when a packaged product is defective, it is necessary to detect most of the causes of chip failure through comparative measurement, expansion of test volume, batch testing and other means of limited comparison. However, the problem that still exists is that it is impossible to accurately determine whether it is a problem with the package or the chip itself, and many batches need to be compared and tested, with each batch having up to thousands of products, which takes a long time, wastes raw materials, and increases production costs.

[0004] In view of this, it is necessary to improve the failed packaged chip detection method in the prior art to solve the technical problem of being unable to accurately determine the source of chip failure. Summary of the invention

[0005] The purpose of the present invention is to provide a failure analysis method for a packaged chip to solve the above technical problems.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A failure analysis method for a packaged chip, comprising:

[0008] Providing chemical solution and heating it, immersing the packaged chip to be analyzed in the chemical solution, and completing the uncapping process of the packaged chip;

[0009] Select a preset epoxy glass carrier tape, load the uncapped packaged chip onto the carrier tape, and bond the gold balls of the packaged chip;

[0010] Carry out UV glue encapsulation and UV curing treatment on the bonded packaged chips;

[0011] Use a product testing platform suitable for glass carriers to test chips and determine the failure type of the chip based on the test results.

[0012] Optionally, the step of providing and heating a chemical solution, immersing the packaged chip to be analyzed in the chemical solution, and completing the uncapping process of the packaged chip; specifically includes:

[0013] cutting off the marked packaged chip monomer from the packaged product, and pre-processing the marked packaged chip monomer;

[0014] A first chemical reagent is provided and placed on a heating table and heated to 65±5° C. The first chemical reagent is 95% to 99% concentration of fuming nitric acid.

[0015] Immerse the pretreated packaged chip monomer into the first chemical reagent and wait for 30 seconds;

[0016] The packaged chip unit is taken out from the first chemical reagent and placed in pure water for cleaning.

[0017] Optionally, the step of washing the mixture in pure water may further include:

[0018] Providing a second chemical reagent and heating it to 50° C.; the second chemical reagent is ethylenediamine;

[0019] Immerse the packaged chip monomer in the second chemical reagent, wait for 60 seconds and then take out the packaged chip monomer;

[0020] The packaged chip monomer taken out is placed in pure water for one cleaning, and then is cleaned twice by ultrasonic wave to obtain the packaged chip monomer with the cap opened.

[0021] Optionally, after obtaining the packaged chip monomer with the cap removed, the step further includes:

[0022] Perform a visual inspection on the packaged chip unit with the cap removed to preliminarily determine the failure type of the packaged chip unit.

[0023] Optionally, a preset epoxy glass carrier tape is selected, and the packaged chip with the cap removed is loaded onto the carrier tape, and the gold balls of the packaged chip are bonded; specifically, the steps include:

[0024] Provides preset film loading tools;

[0025] Using a preset epoxy glass carrier tape, loading the uncapped packaged chip monomer onto the epoxy glass carrier tape through the chip loading tool to obtain a carrier chip;

[0026] Performing an appearance inspection on the carrier chip, and if the inspection result is abnormal, repairing the carrier chip; if the inspection result is normal, continuing the execution;

[0027] A gold wire with a preset diameter is selected to bond the carrier chip to obtain a simulated packaged chip; wherein the diameter of the gold wire is smaller than the diameter of the gold ball of the carrier chip.

[0028] Optionally, the wafer loading tool comprises a tool body, and a vacuum suction nozzle disposed at the lower end of the tool body;

[0029] An air passage is provided in the tool body along its length, and the air passage is connected to an air source component through an air pipe;

[0030] An opening communicating with the air passage is provided on the side wall of the tool body, and the opening is used to control the vacuum nozzle to be opened or closed.

[0031] Optionally, two side portions of the lower end of the tool body are respectively hinged with clamping claw portions, an elastic member is provided between the two clamping claw portions, and the elastic member is used to drive the two clamping claw portions to rotate in a direction away from each other;

[0032] A limiting collar is sleeved on the outer side of the clamping jaw portion, and the limiting collar is connected to a push block assembly, and the push block assembly is used to push the limiting collar to slide, so as to drive the clamping jaw portion to open or close.

[0033] Optionally, the push block assembly includes a first push block and a second push block;

[0034] The first push block is slidably connected to the opening, and the second push block is slidably connected to the outer side wall of the tool body along a first direction; the first direction is the length direction of the tool body;

[0035] The side wall of the first push block is provided with a first inclined portion, and the second push block is provided with a second inclined portion abutting against the first inclined portion;

[0036] The first pushing block is driven to slide along the opening to push the second pushing block to move along the first direction.

[0037] Optionally, judging the failure type of the chip according to the test result specifically includes:

[0038] According to the test results, if the test result shows that the chip is normal, it is a flip-chip failure; if the test result shows that the chip is abnormal, it is a chip body failure.

[0039] Compared with the prior art, the present invention has the following beneficial effects: during detection, the packaged chip is first decapped by heated chemical solution to remove the glue on the chip surface, thereby separating the chip body from the carrier; a preset epoxy glass carrier tape is selected, and the decapped packaged chip is loaded onto the carrier tape, the gold balls of the packaged chip are bonded, and UV glue encapsulation and UV curing treatment are performed to obtain a simulated packaged chip, and the chip is tested. If the chip test result is normal, it is judged that the carrier is defective; if the chip test result is abnormal, it is judged that the chip body is defective; the failure analysis method can avoid damage to the chip function through a non-destructive decapping process, thereby obtaining more accurate and comprehensive analysis data; by selecting a specific carrier tape to load the chip and perform bonding, the packaged chip is simulated, so that the failure type of the problem chip is detected in a targeted manner according to the test result, the repetition of the comparison experiment group and the waste of qualified chips are reduced, the detection efficiency is improved, and it is beneficial to save production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0041] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantive technical significance. Any structural modification, change in proportion or adjustment of size, without affecting the effects and purposes that can be achieved by the present invention, should still fall within the scope of the technical contents disclosed by the present invention.

[0042] Figure 1 It is a schematic diagram of the structure of a flip chip in the background technology;

[0043] Figure 2 is a schematic flow chart of the failure analysis method in this embodiment;

[0044] Figure 3 is a flow chart of step S1 of the failure analysis method in this embodiment;

[0045] Figure 4 Schematic diagram of the process of step S2 of the failure analysis method in this embodiment. DETAILED DESCRIPTION

[0046] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] In the description of the present invention, it should be understood that the terms "upper", "lower", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. It should be noted that when a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a centrally arranged component at the same time.

[0048] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0049] An embodiment of the present invention provides a failure analysis method for a packaged chip, comprising:

[0050] S1, providing chemical solution and heating it, immersing the packaged chip to be analyzed in the chemical solution, and completing the uncapping process of the packaged chip.

[0051] In this step S1, the decapping process is a key process, which uses chemicals to separate the chip body from its carrier tape and remove the glue and gold balls at the same time, so as to obtain an undamaged chip body, providing a basis for further analysis and testing.

[0052] S2, select a preset epoxy glass carrier tape, load the uncapped packaged chip onto the carrier tape, and bond the gold balls of the packaged chip.

[0053] This step S2 involves reloading the processed chip and performing gold ball bonding. By using a pre-set epoxy glass carrier tape, we are able to precisely position and fix the chip, keeping it stable during further packaging and testing.

[0054] S3, performing UV glue encapsulation and UV curing treatment on the bonded packaged chips.

[0055] This step S3 is a secondary packaging and curing process for the bonded chip. By using UV glue and UV curing process, it can ensure that the newly packaged chip has good stability and durability, creating a stable environment for subsequent testing.

[0056] S4, use a product testing platform suitable for glass carriers to test the chip and determine the failure type of the chip based on the test results.

[0057] On a test platform adapted to a specific carrier, functional tests can be systematically performed, and the failure type of the chip can then be accurately determined based on the test results.

[0058] The working principle of the present invention is as follows: during detection, the packaged chip is first decapped by heated chemical solution to remove the glue on the chip surface, thereby separating the chip body from the carrier; a preset epoxy glass carrier tape is selected, and the decapped packaged chip is loaded onto the carrier tape, the gold balls of the packaged chip are bonded, and UV glue encapsulation and UV curing treatment are performed to obtain a simulated packaged chip, and the chip test is performed. If the chip test result is normal, it is judged that the carrier is defective; if the chip test result is abnormal, it is judged that the chip body is defective; compared with the failed packaged chip detection method in the prior art, the failure analysis method can detect the complete process of packaged chips from processing, loading, packaging, testing to failure type judgment, and avoids damage to chip functions through a non-destructive decapping process, so that more accurate and comprehensive analysis data can be obtained; by selecting a specific carrier tape to load the chip and perform bonding to simulate the packaged chip, the failure type of the problem chip is detected in a targeted manner according to the test result, the repetition of the comparison experiment group and the waste of qualified chips are reduced, the detection efficiency is improved, and it is beneficial to save production costs.

[0059] In this embodiment, step S1 specifically includes:

[0060] S11, cutting off the marked packaged chip monomer from the packaged product, and pre-processing the marked packaged chip monomer; cutting off a single packaged product to be analyzed, and pre-processing to remove as much back metal part as possible without causing damage to the chip.

[0061] S12, providing a first chemical reagent, and placing it on a heating table and heating it to 65±5°C; the first chemical reagent is 95%~99% concentration of fuming nitric acid, which is a strong oxidant that can corrode and remove the glue on the packaged chip.

[0062] S13, immersing the pretreated packaged chip monomer into the first chemical reagent and waiting for 30 seconds; this time period is to allow the fuming nitric acid to have enough time to corrode and remove the glue.

[0063] S14, taking out the packaged chip monomer from the first chemical reagent and putting it into pure water for cleaning; in order to remove the fuming nitric acid remaining on the chip and the corroded waste liquid.

[0064] S15, providing a second chemical reagent and heating it to 50° C.; the second chemical reagent is ethylenediamine; ethylenediamine is a strong base, and its main function here is to perform corrosion treatment on the gold balls of the packaged chip.

[0065] S16, immersing the packaged chip monomer into the second chemical reagent, and taking out the packaged chip monomer after waiting for 60 seconds; this step can ensure that ethylenediamine has enough time to corrode and remove the gold ball. The strong alkalinity of ethylenediamine causes the gold ball to corrode and be removed.

[0066] S17, the packaged chip monomer is placed in pure water for a first cleaning, and then cleaned again by ultrasonic wave to obtain the packaged chip monomer with the cap removed; this step is mainly to thoroughly clean the chip and remove the residues of ethylenediamine and the corroded gold ball. The use of ultrasonic wave can provide deep cleaning to ensure that there is no foreign matter on the chip surface.

[0067] S18, perform an appearance inspection on the packaged chip unit with the cap removed to preliminarily determine the failure type of the packaged chip unit. Use a microscope to check its integrity. The surface of the intact product chip has no damage after the above process. If there is any damage, it can be determined based on the morphology whether it is caused by the chip itself or the packaging.

[0068] In this embodiment, step S2 specifically includes:

[0069] S21 provides preset chip loading tools; epoxy glass carrier tape is used, and homemade manual chip loading tools are used. The head of the manual chip loading tool is equipped with a rubber suction nozzle to avoid chip damage during loading. The vacuum is connected to the vacuum tube. The switch is directly on the tool. When the finger blocks the small hole, the suction nozzle has vacuum, and when the finger is released, the suction nozzle has no vacuum.

[0070] S22, using a preset epoxy glass carrier tape, and loading the uncapped packaged chip monomer onto the epoxy glass carrier tape by a chip loading tool to obtain a carrier chip;

[0071] S23, performing appearance inspection on the carrier chip, if the inspection result is abnormal, repairing the carrier chip; if the inspection result is normal, continue to execute;

[0072] S24, selecting a gold wire of a preset diameter to bond the carrier chip to obtain a simulated packaged chip; wherein the diameter of the gold wire is smaller than the diameter of the gold ball of the carrier chip.

[0073] When using gold wire for wire bonding, it depends on the original gold ball. A smaller gold ball than the one after the cap is opened is used as the first wire bonding ball. For example, a 70um ball diameter is used in the original wire bonding. Considering the flattened gold ball remaining after the cap is opened, for example, the diameter of the remaining ball after the cap is opened is 80 microns, a gold ball with a diameter of 55 microns is used for re-wire bonding to ensure the firmness of the ball.

[0074] In this embodiment, the failure type of the chip is determined according to the test results; specifically, the following steps are performed:

[0075] According to the test results, if the test result shows that the chip is normal, it is a flip-chip failure; if the test result shows that the chip is abnormal, it is a chip body failure.

[0076] In this example, the loading tool includes a tool body and a vacuum suction nozzle arranged at the lower end of the tool body; an air path channel is opened in the tool body along its length direction, and the air path channel is connected to an air source component through an air pipe; an opening connected to the air path channel is opened on the side wall of the tool body, and the opening is used to control the opening or closing of the vacuum suction nozzle.

[0077] During operation, the vacuum nozzle is controlled to open or close by operating the opening, so as to facilitate the suction or placement of the packaged chip, so as to facilitate the loading of the chip body onto the epoxy glass carrier.

[0078] Further explanation: the two sides of the lower end of the tool body are respectively hinged with clamping jaws, and an elastic member is arranged between the two clamping jaws, which are used to drive the two clamping jaws to rotate in the direction away from each other; a limiting ring is provided on the outer side of the clamping jaws, and the limiting ring is connected to a push block assembly, which is used to push the limiting ring to slide, so as to drive the clamping jaws to open or close.

[0079] As a preferred solution in this scheme, in order to provide stability during chip loading, the chip body is clamped by a controllable clamping claw to avoid chip deviation during loading.

[0080] Specifically, the push block assembly includes a first push block and a second push block; the first push block is slidably connected to the opening, and the second push block is slidably connected to the outer wall of the tool body along a first direction; the first direction is the length direction of the tool body; the side wall of the first push block is provided with a first inclined portion, and the second push block is provided with a second inclined portion abutting against the first inclined portion; the first push block is driven to slide along the opening to push the second push block to move along the first direction.

[0081] It should be noted that a clamping jaw limiting structure is specifically disclosed, which drives the limiting ring to slide along the outer wall of the clamping jaw by pushing the second pushing block through the first pushing block, so that the clamping jaw can be opened or closed under the action of the elastic member.

[0082] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A failure analysis method for a packaged chip, characterized in that: include: Providing chemical solution and heating it, immersing the packaged chip to be analyzed in the chemical solution, and completing the uncapping process of the packaged chip; Select a preset epoxy glass carrier tape, load the uncapped packaged chip onto the carrier tape, and bond the gold balls of the packaged chip; Carry out UV glue encapsulation and UV curing treatment on the bonded packaged chips; Use a product testing platform suitable for glass carriers to test chips and determine the failure type of the chip based on the test results; The method comprises: selecting a preset epoxy glass carrier tape, loading the uncapped packaged chip onto the carrier tape, and bonding the gold balls of the packaged chip; specifically comprising: Provides preset film loading tools; Using a preset epoxy glass carrier tape, loading the uncapped packaged chip monomer onto the epoxy glass carrier tape through the chip loading tool to obtain a carrier chip; Performing an appearance inspection on the carrier chip, and if the inspection result is abnormal, repairing the carrier chip; if the inspection result is normal, continuing the execution; A gold wire with a preset diameter is selected to bond the carrier chip to obtain a simulated packaged chip; wherein the diameter of the gold wire is smaller than the diameter of the gold ball of the carrier chip.

2. The failure analysis method of packaged chip according to claim 1, characterized in that: The step of providing and heating chemical solution, immersing the packaged chip to be analyzed in the chemical solution, and completing the uncapping process of the packaged chip specifically includes: cutting off the marked packaged chip monomer from the packaged product, and pre-processing the marked packaged chip monomer; Providing a first chemical reagent and placing it on a heating table and heating it to 65±5° C.; the first chemical reagent is 95% to 99% concentration of fuming nitric acid; Immerse the pretreated packaged chip monomer into the first chemical reagent and wait for 30 seconds; The packaged chip unit is taken out from the first chemical reagent and placed in pure water for cleaning.

3. The failure analysis method of packaged chip according to claim 2, characterized in that: The method further comprises: Providing a second chemical reagent and heating it to 50° C.; the second chemical reagent is ethylenediamine; Immerse the packaged chip monomer in the second chemical reagent, wait for 60 seconds and then take out the packaged chip monomer; The packaged chip monomer taken out is placed in pure water for one cleaning, and then is cleaned twice by ultrasonic wave to obtain the packaged chip monomer with the cap opened.

4. The failure analysis method of packaged chip according to claim 3, characterized in that: The step of obtaining the packaged chip monomer with the cap removed further includes: Perform a visual inspection on the packaged chip unit with the cap removed to preliminarily determine the failure type of the packaged chip unit.

5. The failure analysis method of packaged chip according to claim 1, characterized in that: The wafer loading tool comprises a tool body and a vacuum suction nozzle arranged at the lower end of the tool body; An air passage is provided in the tool body along its length, and the air passage is connected to an air source component through an air pipe; An opening communicating with the air passage is provided on the side wall of the tool body, and the opening is used to control the vacuum nozzle to be opened or closed.

6. The failure analysis method of packaged chip according to claim 5, characterized in that: The two sides of the lower end of the tool body are respectively hinged with clamping claws, and an elastic member is arranged between the two clamping claws, and the elastic member is used to drive the two clamping claws to rotate in a direction away from each other; A limiting collar is sleeved on the outer side of the clamping jaw portion, and the limiting collar is connected to a push block assembly, and the push block assembly is used to push the limiting collar to slide, so as to drive the clamping jaw portion to open or close.

7. The failure analysis method of packaged chip according to claim 6, characterized in that: The push block assembly includes a first push block and a second push block; The first push block is slidably connected to the opening, and the second push block is slidably connected to the outer side wall of the tool body along a first direction; the first direction is the length direction of the tool body; The side wall of the first push block is provided with a first inclined portion, and the second push block is provided with a second inclined portion abutting against the first inclined portion; The first pushing block is driven to slide along the opening to push the second pushing block to move along the first direction.

8. The failure analysis method of packaged chip according to claim 1, characterized in that: Determining the failure type of the chip according to the test results specifically includes: According to the test results, if the test result shows that the chip is normal, it is a flip-chip failure; if the test result shows that the chip is abnormal, it is a chip body failure.