Lithium aluminum silicon glass-ceramic and preparation method thereof

By adjusting the composition of lithium aluminosilicate glass and using a 3D hot bending molding process, combined with surface modification treatment, the problems of insufficient mechanical strength and transmittance of lithium aluminosilicate glass-ceramics are solved, achieving high mechanical strength and excellent optical properties.

CN117819824BActive Publication Date: 2024-10-01CHANGSHU JIAHE DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410047409.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-10-10
Filing Date
2024-01-12
Publication Date
2024-10-01
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

Traditional lithium aluminum silicon-ceramic glass has deficiencies in mechanical strength and transmittance, which limits its application in the field of electronic products.

Method used

By adjusting the proportion of the main components and auxiliary components of lithium aluminosilicate glass, a 3D hot bending molding process is adopted, and the glass surface is modified, including using V2O5 and Ta2O5 composite nucleating agents, Sb2O3, SnO2 and Fe2O3 clarifiers, Nd2O3, Sm2O3 and CeO2 dopants and B2O3 co-solvent are used for multi-step heat treatment and surface modification.

Benefits of technology

The flexural strength, transmittance and hydrophobic properties of lithium aluminum silicon-ceramic glass are significantly improved, ensuring its high mechanical strength and optical performance in the field of electronic products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of microcrystalline glass, and discloses a lithium aluminum silicon microcrystalline glass and a preparation method thereof. The addition of V2O5 and Ta2O5 composite nucleating agents reduces the crystallization temperature of the glass and improves the stability of the glass. Doping agents such as CeO2 significantly accelerate the crystal growth rate, so that the glass nucleates and crystallizes at a lower temperature, thereby improving the glass transmittance. Cosolvents such as B2O3 reduce the high-temperature viscosity of the glass, reduce the activation free energy in the crystallization process of the glass, and are beneficial to crystallization and processing. The 3D hot bending process undergoes preheating, pressurizing, annealing and cooling stages, and the copper mold transfers heat to the glass by heat conduction, so that the glass is evenly heated during the heating process, and natural cooling can prevent breakage or inaccurate dimensional accuracy caused by excessive cooling. The glass surface is grafted and modified, so that the hydrophobicity of the glass is significantly improved, so that the glass has excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microcrystalline glass, and in particular to a lithium aluminum silicon microcrystalline glass and a preparation method thereof. Background Art

[0002] Glass-ceramics, also known as glass ceramics, consists of a microcrystalline phase and a glass phase, and has the dual characteristics of glass and ceramics. Therefore, glass-ceramics are widely used in daily life. However, traditional glass is relatively brittle and prone to microcracks, making its actual mechanical strength lower than the theoretical mechanical strength, thus limiting the application of glass-ceramics in some fields. With the popularization of electronic products, the requirements for glass transparency are getting higher and higher, so glass-ceramics must have higher optical transmittance and higher mechanical strength. Therefore, modifying glass-ceramics to meet its application in the field of electronic products has become an urgent problem for technicians to solve.

[0003] Lithium aluminum silicate glass is made of SiO2, Al2O3 and Li2O as main components, and a certain amount of nucleating agent, cosolvent and other auxiliary components are added to melt. The main components are the basis for preparing microcrystalline glass, and the auxiliary components are used to adjust the performance of the glass. Therefore, to obtain microcrystalline glass with ideal physical properties, it is necessary to strictly control the proportion of each component and the content of the auxiliary components. Patent CN102167507B discloses thin lithium aluminum silicate glass for 3D tight molding, wherein the corresponding raw materials such as SiO2, Al2O3 and Li2O are mixed, melted and kept warm in a platinum crucible, and then clarified, and the glass melt is poured into a cold stainless steel mold to obtain a bulk glass, and then the glass is annealed, cut, edged, and finely planed into the required sample size, to prepare a glass that can be chemically tempered and easy to 3D mold. However, simple cutting and edge grinding cannot meet the requirements of glass 3D molding accuracy, and tensile stress will be formed in the center of the glass during pressing. Excessive tensile stress will increase the risk of glass breakage. The present invention adjusts the ratio of the main component and the auxiliary component of the lithium aluminum silicate glass, performs 3D hot bending on the glass, and then performs surface modification, so that the prepared glass has high mechanical strength and transmittance. Summary of the invention

[0004] The technical problem solved by the present invention is: to provide a lithium aluminum silicon microcrystalline glass and a preparation method thereof, thereby solving the problem of insufficient strength and low transmittance of the lithium aluminum silicon microcrystalline glass.

[0005] The technical solution of the present invention is:

[0006] A method for preparing lithium aluminum silicon glass-ceramics, the glass-ceramics comprising the following components: 55-75 parts by weight of SiO2, 1-12 parts of Al2O3, 9-15 parts of Li2O, 2-6 parts of P2O5, 3-12 parts of ZrO2, 3-6 parts of composite nucleating agent, 0.1-8 parts of Na2O, 0.1-0.2 parts of K2O, 0.2-0.3 parts of ZnO, 0.1-0.3 parts of MgO, 2-10 parts of CaO, 1-3 parts of B2O3, 2-5 parts of Y2O3, 0.01-0.5 parts of clarifier, 0.3-0.9 parts of dopant and 0.4-1.6 parts of solvent; the preparation method is carried out according to the following steps:

[0007] (1) After the above glass components are fully mixed, they are placed in a corundum crucible, heated to 1600-1650°C at 5-10°C / min in a silicon-molybdenum furnace and melted for 3-7 hours. After clarification, the glass liquid is cast on a preheated copper mold, and the formed glass is placed in a muffle furnace at 550-600°C and kept warm for 1-3 hours for annealing and cooling to obtain a basic glass; the basic glass is heated to 580-600°C at 5-10°C / min, kept warm for 2-3 hours for nucleation, and then heated to 700-750°C at 10-15°C, kept warm for 2-4 hours for crystallization to obtain a basic microcrystalline glass.

[0008] (2) A heating tube with a diameter of 15-20 mm and a power of 10-15 kW is used for interference fit on the upper and lower heating plates for heating, and the basic microcrystalline glass is placed in a copper mold. Four groups of molding temperatures are set respectively, and the copper mold containing the basic glass is kept warm at different molding temperatures to keep the temperature inside the glass uniform. First, the upper and lower heating plates are heated to the first group of molding temperatures and kept warm for a certain period of time. Then, the copper mold is moved to the heating molding area, heated to the second group of molding temperatures, kept warm for a certain period of time, and vacuumed to obtain curved glass; then, the copper mold is moved to the first annealing area, cooled to the third group of molding temperatures, and kept warm for a period of time; finally, the mold is moved to the hot pressing molding area, heated to the fourth group of molding temperatures, and kept warm for a period of time. At the preset pressure and molding rate, the upper and lower molds are moved in unison, and hot pressing molding is performed in a nitrogen atmosphere, and the temperature is naturally cooled to obtain lithium aluminum silicon microcrystalline glass.

[0009] Furthermore, in the step (1), the composite nucleating agent is V2O5 and Ta2O5, and the mass ratio of V2O5:Ta2O5 is 1-1.5:2-4.5.

[0010] Furthermore, the clarifier in step (1) is any one of Sb2O3, SnO2 or Fe2O3.

[0011] Furthermore, the dopant in step (1) is any one of Nd2O3, Sm2O3 or CeO2.

[0012] Furthermore, the co-solvent in step (1) is B2O3.

[0013] Furthermore, in the step (2), the four groups of molding temperatures are 720-770°C, 700-750°C, 680-730°C and 750-810°C respectively.

[0014] Furthermore, in step (2), the insulation time of the first group is 60-150s, the insulation time of the second group is 50-150s, the insulation time of the third group is 80-160s, and the insulation time of the fourth group is 90-150s.

[0015] Furthermore, in the step (2), the preset pressure is 0.3-0.5 MPa, and the preset molding speed is 1.25-1.75 mm / min.

[0016] Furthermore, a modification method for the lithium aluminum silicon glass-ceramics prepared by the above preparation method is provided, wherein the modification method is:

[0017] S1. Wipe both sides of the lithium aluminum silicon glass-ceramics with absorbent cotton soaked in ethanol, cut into a certain size, ultrasonically treat in a beaker containing deionized water, ethanol and acetone for 15-25 minutes, blow dry with nitrogen, and then place in a 98% concentrated sulfuric acid and 30% hydrogen peroxide solution with a volume ratio of 5-7:3, and then soak in a water bath at 90-100℃ for 1-3 hours. Take out the lithium aluminum silicon glass-ceramics, wash with deionized water, and dry to obtain surface hydroxylated glass.

[0018] S2. Immerse the surface hydroxylated glass-ceramics in a toluene solution of trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane at a certain concentration, adjust the pH to 3-5 with acetic acid, let it stand for 24-36 hours, wash with ethanol, and dry to obtain modified lithium aluminum silicon glass-ceramics.

[0019] Furthermore, in step S2, the concentration of the toluene solution of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane is 0.8-1.6 mg / mL.

[0020] Furthermore, a lithium aluminum silicon microcrystalline glass may also include the following raw materials in weight: 55-75 parts SiO2, 1-12 parts Al2O3, 9-15 parts LiO2, 2-6 parts P2O5, 3-12 parts ZrO2, 0.1-8 parts Na2O, 0-0.5 parts K2O, 0-0.5 parts ZnO, 0-0.5 parts MgO, 0-10 parts CaO, 0-3 parts B2O3, 0-5 parts Y2O3, 0.01-0.5% Sb2O3, 0.01-0.5% SnO2. The content of lithium disilicate in the microcrystalline glass phase is ≥ 20%, and the content of lithium disilicate crystals is determined by X-ray diffractometer testing, and the test results are compared with the standard PDF card analysis to obtain the corresponding crystal phase in the microcrystalline glass, and the corresponding crystallinity is calculated.

[0021] Furthermore, the transmittance of the lithium aluminum silicon glass-ceramics in the ultraviolet-visible light range of 200-800nm ​​at a thickness of 2mm can reach up to 85.3%. In some embodiments, the transmittance of the ultraviolet-visible light in the wavelength range of 200-800nm ​​is 73%-85%.

[0022] Furthermore, the corrosion resistance of the lithium aluminum silicon glass-ceramics was tested in 20% by mass sodium hydroxide and sulfuric acid solutions respectively: the alkaline weight loss rate of the lithium aluminum silicon glass-ceramics did not exceed 0.9%, and the acidic weight loss rate did not exceed 1.95%, wherein the weight loss rate = (initial mass of the glass sample - mass of the glass sample after corrosion) / initial mass of the glass sample; in some embodiments, the alkaline weight loss rate of the lithium aluminum silicon glass-ceramics was 0.6%-0.9%, and the acidic weight loss rate was 1%-1.95%.

[0023] Furthermore, the flexural strength of the lithium aluminum silicon glass-ceramics is not less than 90 MPa. In some embodiments, the flexural strength is 90-96 MPa.

[0024] Furthermore, the lithium aluminum silicon glass-ceramics has good hydrophobicity. The hydrophobicity of the glass surface is tested using an optical contact angle meter. The contact angles at three different positions of the glass are tested and the average value is taken. The contact angle is 97°-122°.

[0025] The beneficial technical effects of the present invention are:

[0026] (1) The present invention first adjusts the ratio of the main components in the lithium aluminum silicate glass-ceramics, and then adds auxiliary components such as a clarifier, a composite nucleating agent, a dopant and a co-solvent while ensuring the glass-ceramic network structure, so that the components play a synergistic role. Then, the glass is subjected to multiple steps of 3D hot bending treatment to improve the flexural strength of the glass. Finally, the surface of the lithium aluminum silicate glass is modified, and the obtained lithium aluminum silicate glass has good hydrophobicity.

[0027] (2) Adding V2O5 and Ta2O5 composite nucleating agents lowers the crystallization temperature of the glass and improves the stability of the glass. Adding clarifiers such as Sb2O3, SnO2 and Fe2O3 absorbs oxygen at low temperatures and decomposes and releases oxygen at high temperatures, which plays a clarifying role. The addition of co-solvent B2O3 reduces the high-temperature viscosity of the glass, which reduces the activation free energy during the crystallization process, which is beneficial to crystallization and processing. Adding dopants such as Nd2O3, Sm2O3 and CeO2 significantly accelerates the crystal growth rate, allowing the glass to nucleate and crystallize at a lower temperature. 4+ Ions and Nd 3+ The ions are network interstitial ions. The pinning effect of the ions makes the glass network tighter, diffusion more difficult, and has a certain grain refinement effect, thereby improving the thermal stability of the microcrystalline glass and increasing the transmittance of the glass.

[0028] (3) The 3D hot bending process goes through the preheating, pressurizing, annealing and natural cooling stages. The copper mold transfers heat to the glass through heat conduction, so that the glass is heated evenly during the heating process with a small temperature difference. Natural cooling is used to reduce the internal stress of the finished glass caused by the molding rate problem, and can prevent breakage or dimensional inaccuracy caused by excessive cooling. The glass surface is grafted and modified, which significantly improves the hydrophobicity of the glass, making the prepared lithium aluminum silicon glass-ceramics have excellent comprehensive performance. Implementation

[0029] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention. Example 1

[0030] (1) 75 parts of SiO2, 1 part of Al2O3, 10 parts of Li2O, 3 parts of P2O5, 5 parts of ZrO2, 1.2 parts of V2O5, 2.3 parts of Ta2O5, 0.9 parts of Na2O, 0.1 parts of K2O, 0.25 parts of ZnO, 0.15 parts of MgO, 8 parts of CaO, 3 parts of B2O3, 2 parts of Y2O3, 0.2 parts of Sb2O3, 0.7 parts of CeO2 and 0.4 parts of B2O3 were mixed thoroughly. After homogenization, place it in a corundum crucible, heat it to 1620℃ at 8℃ / min in a silicon-molybdenum furnace and melt it for 5h. After clarification, cast the glass liquid on a preheated copper mold, and put the formed glass into a muffle furnace at 560℃ and keep it for 2h for annealing and cooling to obtain basic glass; heat the basic glass to 600℃ at 5℃ / min, keep it for 3h for nucleation, and then heat it to 720℃ at 125℃, keep it for 4h for crystallization to obtain basic microcrystalline glass.

[0031] (2) A heating tube with a diameter of 15 mm and a power of 12 kW was used for interference fit on the upper and lower heating plates for heating. The basic microcrystalline glass was placed in a copper mold. Four groups of molding temperatures were set respectively. The copper mold containing the basic glass was kept warm at different molding temperatures to keep the temperature inside the glass uniform. First, the upper and lower heating plates were heated to 730°C and kept warm for 80 seconds. Then, the copper mold was moved to the heating molding area, heated to 750°C, kept warm for 110 seconds, and vacuumed to obtain curved glass. Then, the copper mold was moved to the first annealing area, cooled to 720°C, and kept warm for 150 seconds. Finally, the mold was moved to the hot pressing molding area, heated to 800°C, and kept warm for 120 seconds. At a preset pressure of 0.5 MPa and a molding rate of 1.5 mm / min, the upper and lower molds were moved in a matching manner. Hot pressing molding was carried out in a nitrogen atmosphere, and the temperature was naturally cooled to obtain lithium aluminum silicon microcrystalline glass.

[0032] (3) Wipe both sides of the lithium aluminum silicon glass-ceramics with absorbent cotton soaked in ethanol, cut into a certain size, ultrasonically treat for 25 min in a beaker containing deionized water, ethanol and acetone, blow dry with nitrogen, and then place in a solution of 98% concentrated sulfuric acid and 30% hydrogen peroxide in a volume ratio of 6:3. Then, soak in a water bath at 95°C for 3 h. Take out the lithium aluminum silicon glass-ceramics, wash with deionized water, and dry to obtain surface hydroxylated glass.

[0033] (4) The surface hydroxylated glass-ceramics was immersed in a toluene solution of trimethoxy (1H,1H,2H,2H-heptadecafluorodecyl) silane with a concentration of 0.8 mg / mL, and the pH was adjusted to 4 with acetic acid. After standing for 32 hours, the glass-ceramics were washed with ethanol and dried to obtain modified lithium aluminum silicon glass-ceramics. Example 2

[0034] The difference between this embodiment and embodiment 1 is that in step (1), SiO2 is 72 parts and Al2O3 is 4 parts, and other conditions remain unchanged. Example 3

[0035] The difference between this embodiment and embodiment 1 is that in step (1), SiO2 is 69 parts and Al2O3 is 7 parts, and other conditions remain unchanged. Example 4

[0036] The difference between this embodiment and embodiment 1 is that in step (1), SiO2 is 66 parts and Al2O3 is 10 parts, and other conditions remain unchanged. Example 5

[0037] The difference between this embodiment and embodiment 1 is that in step (1), SiO2 is 64 parts and Al2O3 is 12 parts, and other conditions remain unchanged. Example 6

[0038] (1) 66 parts by weight of SiO2, 10 parts by weight of Al2O3, 12 parts by weight of Li2O, 5 parts by weight of P2O5, 4 parts by weight of ZrO2, 1.3 parts by weight of V2O5, 4.2 parts by weight of Ta2O5, 2.5 parts by weight of Na2O, 0.2 parts by weight of K2O, 0.2 parts by weight of ZnO, 0.3 parts by weight of MgO, 6 parts by weight of CaO, 2 parts by weight of B2O3, 3.5 parts by weight of Y2O3, 0.3 parts by weight of Sb2O3, 0.5 parts by weight of CeO2 and 0.4 parts by weight of B2O3 were mixed thoroughly. After homogenization, place it in a corundum crucible, heat it to 1650℃ at 10℃ / min in a silicon-molybdenum furnace and melt it for 6h. After clarification, cast the glass liquid on a preheated copper mold, and put the formed glass into a muffle furnace at 600℃ and keep it warm for 1h for annealing and cooling to obtain basic glass; heat the basic glass to 580℃ at 10℃ / min, keep it warm for 3h for nucleation, and then heat it to 740℃ at 12℃, keep it warm for 3h for crystallization to obtain basic microcrystalline glass.

[0039] (2) A heating tube with a diameter of 20 mm and a power of 13 kW was used for interference fit on the upper and lower heating plates for heating. The basic microcrystalline glass was placed in a copper mold. Four groups of molding temperatures were set respectively. The copper mold containing the basic glass was kept warm at different molding temperatures to keep the temperature inside the glass uniform. First, the upper and lower heating plates were heated to 730°C and kept warm for 90 seconds. Then, the copper mold was moved to the heating molding area, heated to 750°C, kept warm for 130 seconds, and vacuumed to obtain curved glass. Then, the copper mold was moved to the first annealing area, cooled to 690°C, and kept warm for 140 seconds. Finally, the mold was moved to the hot pressing molding area, heated to 780°C, and kept warm for 100 seconds. At a preset pressure of 0.4 MPa and a molding rate of 1.75 mm / min, the upper and lower molds were moved in a matching manner, and hot pressing molding was carried out in a nitrogen atmosphere. The mold was naturally cooled to obtain lithium aluminum silicon microcrystalline glass.

[0040] (3) Wipe both sides of the lithium aluminum silicon glass-ceramics with absorbent cotton soaked in ethanol, cut into a certain size, ultrasonically treat for 20 min in a beaker containing deionized water, ethanol and acetone, blow dry with nitrogen, and then place in a solution of 98% concentrated sulfuric acid and 30% hydrogen peroxide in a volume ratio of 7:3. Then, soak in a water bath at 100°C for 2 h, take out the lithium aluminum silicon glass-ceramics, wash with deionized water, and dry to obtain surface hydroxylated glass.

[0041] (4) The surface hydroxylated glass-ceramics was immersed in a toluene solution of trimethoxy (1H,1H,2H,2H-heptadecafluorodecyl) silane with a concentration of 0.8 mg / mL, and the pH was adjusted to 5 with acetic acid. After standing for 24 hours, the glass-ceramics were washed with ethanol and dried to obtain modified lithium aluminum silicon glass-ceramics. Example 7

[0042] The difference between this embodiment and embodiment 6 is that the co-solvent in step (1) is 0.7 parts of B2O3, and other conditions remain unchanged. Example 8

[0043] The difference between this embodiment and embodiment 6 is that the co-solvent in step (1) is 1.0 part of B2O3, and other conditions remain unchanged. Example 9

[0044] The difference between this embodiment and embodiment 6 is that the co-solvent in step (1) is 1.3 parts of B2O3, and other conditions remain unchanged. Example 10

[0045] The difference between this embodiment and embodiment 6 is that the co-solvent in step (1) is 1.6 parts of B2O3, and other conditions remain unchanged. Embodiment 11

[0046] The difference between this embodiment and embodiment 6 is that the concentration of the toluene solution of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane in step (4) is 1.0 mg / mL. Example 12

[0047] The difference between this embodiment and embodiment 6 is that the concentration of the toluene solution of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane in step (4) is 1.2 mg / mL. Embodiment 13

[0048] The difference between this embodiment and embodiment 6 is that the concentration of the toluene solution of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane in step (4) is 1.4 mg / mL. Embodiment 14

[0049] The difference between this embodiment and embodiment 6 is that the concentration of the toluene solution of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane in step (4) is 1.6 mg / mL.

[0050] Comparative Example 1

[0051] The difference between this comparative example and Example 6 is that the composite nucleating agents V2O5 and Ta2O5 are not added in step (1), and other conditions remain unchanged.

[0052] Comparative Example 2

[0053] The difference between this comparative example and Example 6 is that no clarifier Sb2O3 is added in step (1), and other conditions remain unchanged.

[0054] Comparative Example 3

[0055] The difference between this comparative example and Example 6 is that no dopant CeO2 is added in step (1), and other conditions remain unchanged.

[0056] Comparative Example 4

[0057] The difference between this comparative example and Example 6 is that no co-solvent B2O3 is added in step (1), and other conditions remain unchanged.

[0058] Comparative Example 5

[0059] The difference between this comparative example and Example 6 is that the basic microcrystalline glass obtained in step (1) is not subjected to the next step of heat bending treatment.

[0060] Comparative Example 6

[0061] The difference between this comparative example and Example 6 is that the lithium aluminum silicon glass-ceramics obtained in step (2) is not subjected to surface modification treatment.

[0062] Transmittance test: polish both sides of the glass sample to a thickness of 2mm, and use a spectrophotometer to test the UV-visible light transmittance (or transmittance) of the glass in the range of 200-800nm.

[0063] Glass transition temperature (T g ) Test: The glass transition temperature was tested by differential thermal analyzer with a heating rate of 10℃ / min.

[0064] Table 1: Lithium aluminum silicon glass ceramic test table

[0065] Transmittance (%) <![CDATA[T g (℃)]]> Example 1 73.3 662.1 Example 2 76.4 679.2 Example 3 82.8 687.1 Example 4 85.3 693.0 Example 5 83.2 698.4 Comparative Example 1 55.1 645.2 Comparative Example 2 61.0 556.2 Comparative Example 3 63.1 578.3

[0066] It can be seen from the above table that with the increase of Al2O3 content in lithium aluminum silicon glass-ceramics, the content of SiO2 is appropriately reduced under the condition of ensuring the formation of glass network, because when the content of SiO2 is too much, it will lead to difficulties in melting and forming the glass; in Example 4, when the addition amount of SiO2 is 66 parts and Al2O3 is 10 parts, the transmittance of the sample reaches 85.3% at most, indicating that the transmittance of the glass is better at this time, because the ultraviolet absorption of the glass is mainly caused by the excitation of the extranuclear electrons of oxygen ions absorbing photons, and Al2O3 helps to improve the chemical stability of the glass; Comparative Example 1 does not add a composite nucleating agent, resulting in a glass transmittance of only 55.1% The addition of composite nucleating agent is beneficial to the crystallization of glass and increases the transparency; in comparative example 2, no clarifier is added, and the transmittance is 61.0%. The clarifier Sb2O3 and the like play a clarification role in the system, absorbing oxygen at low temperature and decomposing and releasing oxygen at high temperature. Since the clarification temperatures of Sb2O3, SnO2 and Fe2O3 are different, the composite clarifier composed of them can play a better clarification role, thereby improving the transmittance of the glass; in comparative example 3, no dopant is added, and the transmittance is 63.1%. The dopant CeO2 and the like makes the glass network tight and diffusion more difficult, has a certain refining effect on the grains, improves the thermal stability of the microcrystalline glass, and improves the transmittance of the glass.

[0067] The glass transition temperature increases with the increase of Al2O3 content. This is because the increase of chemical bond energy in the glass structure strengthens the glass structure, thereby improving the stability of the glass. The Tg of comparative example 1 is 645.2°C. This is because the composite nucleating agent of V2O5 and Ta2O5 can reduce the forming ability of glass, increase the glass transition temperature, promote crystallization, and make the glass structure tight and firm.

[0068] Acid and alkali resistance test: Prepare 20% NaOH and H2SO4 solution by mass, put the glass sample into the solution for corrosion for 12 hours, take it out and weigh it, and use the weight loss method to determine the acid and alkali resistance of the sample.

[0069] Weight loss rate = (initial mass of glass sample - mass of glass sample after corrosion) / initial mass of glass sample.

[0070] Table 2: Lithium aluminum silicon glass ceramic test table

[0071] Alkaline weight loss rate (%) Acidic weight loss rate (%) Example 1 0.65 1.24 Example 2 0.59 1.60 Example 3 0.90 1.95 Example 4 0.72 1.06 Example 5 0.79 1.35

[0072] High temperature viscosity test: Use a high temperature viscometer to test the glass's high temperature viscosity at 1300°C.

[0073] Table 3: High temperature viscosity test table

[0074] Viscosity (dPa·s) Example 6 657.3 Example 7 581.0 Example 8 538.1 Example 9 481.5 Example 10 420.2 Comparative Example 4 738.3

[0075] It can be seen from the data in the above table that with the increase of the boron content in the lithium aluminum silicon glass-ceramics, the high-temperature viscosity of the glass gradually decreases. The comparative example 4 does not contain a co-solvent and has a viscosity of 738.3 dPa·s, while when the boron addition amount of Example 10 is 1.6 parts, the viscosity is reduced to 420.2 dPa·s, indicating that the introduction of boron can significantly reduce the high-temperature viscosity of the glass. This is because B2O3 replaces silicon oxygen tetrahedron [SiO4] in the form of [BO3], that is, boron ions can replace oxygen ions in the glass network structure, causing the large silicon oxygen tetrahedrons in the glass system to depolymerize, resulting in the matrix glass structure becoming loose and the network connection degree reduced, thereby reducing the viscosity and melting temperature, which is beneficial to the glass forming process.

[0076] Flexural strength test: Use a material testing machine to test the flexural strength of glass.

[0077] Table 4: Flexural strength test table

[0078] Flexural strength (MPa) Example 1 90.1 Example 2 91.9 Example 3 93.2 Example 4 95.6 Example 5 94.4 Comparative Example 5 52.1

[0079] The 3D glass hot bending process is to place the cut glass between the arc-shaped molds of the hot bending machine, heat it to a certain temperature in turn through several workstations to soften the glass, soften the glass under a certain pressure to make it gradually fit the mold, and then cold-cut it by maintaining pressure and gradually cooling it to obtain 3D shaped glass; Comparative Example 5 did not undergo 3D hot bending treatment, and the flexural strength of the glass was only 52.1 MPa, while the flexural strengths of Examples 1-5 were all above 90 MPa, indicating that the hot bending process can significantly improve the strength of the glass; in addition, Al2O3 is an important component for preparing high-strength and high-hardness glass. Therefore, as the Al2O3 content increases, the glass has a larger space as a channel for ion exchange, and the glass strength is increased.

[0080] Contact angle test: Use an optical contact angle meter to test the hydrophobicity of the glass surface. Test the contact angles at three different positions on the glass and take the average value.

[0081] Table 5: Contact angle test table

[0082] Contact angle (°) Example 6 97.3 Embodiment 11 105.4 Example 12 113.3 Example 13 118.5 Embodiment 14 122.0 Comparative Example 6 84.2

[0083] The monomer containing fluorine element is a material with very low surface energy. As the concentration of fluorine-containing monomer on the surface of lithium aluminum silicon microcrystalline glass increases, the grafting rate of glass to fluorine monomer increases, thereby increasing the contact angle of the glass surface and enhancing the hydrophobicity. In Example 6, the glass surface was not fluorine-modified, and its contact angle was 84.2°, while the contact angle of Example 14 reached 122.0°, so the hydrophobicity of the glass was greatly improved. Although the above describes the specific implementation of the present invention, it is not a limitation on the protection scope of the present invention. Based on the technical solution of the present invention, various modifications or deformations that can be made by those skilled in the art without creative labor are still within the protection scope of the present invention.

Claims

1. A method for preparing lithium aluminum silicon glass-ceramics, characterized in that: The microcrystalline glass comprises the following components: by weight: 55-75 parts of SiO2, 1-12 parts of Al2O3, 9-15 parts of Li2O, 2-6 parts of P2O5, 3-12 parts of ZrO2, 3-6 parts of composite nucleating agent, 0.1-8 parts of Na2O, 0.1-0.2 parts of K2O, 0.2-0.3 parts of ZnO, 0.1-0.3 parts of MgO, 2-10 parts of CaO, 1-3 parts of B2O3, 2-5 parts of Y2O3, 0.01-0.5 parts of a clarifier, 0.3-0.9 parts of a dopant and 0.4-1.6 parts of a flux, wherein the composite nucleating agent is V2O5 and Ta2O5, and the mass ratio is V2O5:Ta2O5=1-1.5:2-4.5; the clarifier is any one of Sb2O3, SnO2 or Fe2O3; the dopant is any one of Nd2O3, Sm2O3 or CeO2; the flux is B2O3; The preparation method is carried out according to the following steps: Step (1) After the above-mentioned microcrystalline glass components are fully mixed and uniformly mixed, the mixture is placed in a corundum crucible, and the mixture is heated to 1600-1650°C at a rate of 5-10°C / min in a silicon-molybdenum furnace and melted for 3-7 hours. After clarification, the glass liquid is cast on a preheated copper mold, and the formed glass is placed in a muffle furnace at 550-600°C and kept warm for 1-3 hours for annealing and cooling to obtain a basic glass; the basic glass is heated to 580-600°C at a rate of 5-10°C / min, kept warm for 2-3 hours for nucleation, and then heated to 700-750°C at a rate of 10-15°C, and kept warm for 2-4 hours for crystallization to obtain a basic microcrystalline glass; Step (2) uses a heating tube with a diameter of 15-20 mm and a power of 10-15 kW to heat on the upper and lower heating plates through interference fit, places the basic microcrystalline glass in a copper mold, sets four groups of molding temperatures respectively, and keeps the copper mold containing the basic glass at different molding temperatures to keep the temperature inside the glass uniform. First, the upper and lower heating plates are heated to the first group of molding temperatures and kept warm for a certain period of time. Then, the copper mold is moved to the heating and molding area, heated to the second group of molding temperatures, kept warm for a certain period of time, and vacuumed to obtain curved glass; then, the copper mold is moved to the first annealing area, cooled to the third group of molding temperatures, and kept warm for a period of time; finally, the mold is moved to the hot pressing molding area, heated to the fourth group of molding temperatures, and kept warm for a period of time. At a preset pressure and molding rate, the upper and lower molds are moved in a matching manner, and hot pressing molding is performed in a nitrogen atmosphere, and the temperature is naturally cooled to obtain lithium aluminum silicon microcrystalline glass.

2. The method for preparing lithium aluminum silicon glass-ceramics according to claim 1, characterized in that: The four groups of molding temperatures in step (2) are 720-770°C, 700-750°C, 680-730°C and 750-810°C respectively.

3. The method for preparing lithium aluminum silicon glass-ceramics according to claim 1, characterized in that: In step (2), the insulation time of the first group is 60-150s, the insulation time of the second group is 50-150s, the insulation time of the third group is 80-160s, and the insulation time of the fourth group is 90-150s.

4. The method for preparing lithium aluminum silicon glass-ceramics according to claim 1, characterized in that: In the step (2), the preset pressure is 0.3-0.5 MPa, and the preset molding speed is 1.25-1.75 mm / min.

5. A method for modifying the lithium aluminum silicon glass-ceramics obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The modification method is: S1. Wipe both sides of the lithium aluminum silicon glass-ceramics with absorbent cotton soaked in ethanol, cut into a certain size, ultrasonicate in a beaker containing deionized water, ethanol and acetone for 15-25 minutes, blow dry with nitrogen, and then place in a 98% mass fraction of concentrated sulfuric acid and a 30% mass fraction of hydrogen peroxide solution with a volume ratio of 5-7:3, and then soak in a water bath at 90-100°C for 1-3 hours, take out the lithium aluminum silicon glass-ceramics, wash with deionized water, and dry to obtain surface hydroxylated glass; S2. Immerse the surface hydroxylated glass-ceramics in a toluene solution of a certain concentration of trimethoxy-1H,1H,2H,2H-heptadecafluorodecyl-silane, adjust the pH to 3-5 with acetic acid, let it stand for 24-36 hours, wash with ethanol, and dry to obtain modified lithium aluminum silicon glass-ceramics.

6. The method for modifying lithium aluminum silicon glass-ceramics according to claim 5, characterized in that: The concentration of the toluene solution of trimethoxy-1H,1H,2H,2H-heptadecafluorodecyl-silane in step (2) is 0.8-1.6 mg / mL.