A multifunctional polylactic acid textile containing chlorogenic acid and preparation method thereof

Multifunctional PLA fibers and nonwoven materials were prepared by melt blending chlorogenic acid and polylactic acid, which solved the problems of resource shortage and low functionalization, and achieved antioxidant and ultraviolet shielding effects, meeting the needs of healthy textiles.

CN117822144BActive Publication Date: 2024-10-01JIANGNAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311827098.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-01
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

In the current technology, chlorogenic acid and polylactic acid have not been combined to prepare textiles, which affects their respective properties. Furthermore, synthetic fibers and spunbond nonwoven materials suffer from resource shortages and low levels of functionalization.

Method used

Multifunctional PLA fibers or nonwoven materials are prepared by melt blending and granulating chlorogenic acid and polylactic acid, maintaining the physical and mechanical properties of PLA and introducing the antioxidant and UV shielding functions of chlorogenic acid.

Benefits of technology

The prepared multifunctional PLA fibers and nonwoven materials retain the spinnability and mechanical properties of PLA, while also possessing antioxidant and UV shielding functions, meeting the needs of healthy textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004635438120000041
    Figure BDA0004635438120000041
Patent Text Reader

Abstract

The invention discloses a multifunctional polylactic acid textile containing chlorogenic acid and a preparation method thereof, and belongs to the field of functional fiber and nonwoven material preparation. The invention firstly blends CGA and PLA into granules; then performs melt spinning or spunbond nonwoven processing to prepare multifunctional PLA fiber or multifunctional PLA nonwoven material. The invention uses natural extract CGA as a functional factor, has anti-ultraviolet and ultraviolet shielding functions, has a melting point of about 210°C, which is close to the melting point of PLA, is suitable for melt blending with PLA to prepare multifunctional PLA fiber or multifunctional PLA nonwoven material, while maintaining the physical and mechanical properties of the PLA fiber itself.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multifunctional polylactic acid textile containing chlorogenic acid and a preparation method thereof, belonging to the field of preparation of functional fibers and nonwoven materials. Background Art

[0002] The raw materials of synthetic fibers and spunbond nonwoven materials are mainly petroleum-based polymer materials, which have problems such as resource shortage and environmental pollution; polylactic acid (PLA) is a resource-renewable, biodegradable thermoplastic polymer material that can be melt-processed. It can replace petroleum-based polymer materials as the raw materials of synthetic fibers and spunbond nonwoven materials to overcome the current problems of resource shortage and environmental pollution in the field of synthetic fibers and spunbond nonwoven materials. In addition, although the output of synthetic fibers and nonwoven materials is high, their functionalization degree is very low, which makes it difficult to meet people's demand for functionalization; especially, with the improvement of living standards, people's demand for healthy textiles is increasing.

[0003] Chlorogenic acid (CGA) is a natural functional material extracted from plants such as honeysuckle and eucommia. It has antioxidant and UV shielding functions and is non-toxic. It can remove active free radicals on the skin surface and prevent skin aging. It can absorb ultraviolet light of 280 to 400 nm and protect the skin from damage by ultraviolet rays.

[0004] However, so far, no one has found that chlorogenic acid is used in PLA. Summary of the invention

[0005] [Technical issues]

[0006] CGA has excellent performance and PLA resources are renewable, but there is no literature mentioning how to combine the two for spinning or fabric preparation without affecting their respective properties.

[0007] [Technical solution]

[0008] In order to solve the above problems, the present invention firstly blends CGA and PLA into granules; then performs melt spinning or spunbond nonwoven processing to prepare multifunctional PLA fiber or multifunctional PLA nonwoven material. The present invention uses natural extract CGA as a functional factor, has anti-ultraviolet and ultraviolet shielding functions, has a melting point of about 210°C, which is close to the melting point of PLA, is suitable for melt blending with PLA to prepare multifunctional PLA fiber or multifunctional PLA nonwoven material, while maintaining the physical and mechanical properties of the PLA fiber itself.

[0009] The first object of the present invention is to provide a method for preparing a multifunctional polylactic acid textile containing chlorogenic acid, comprising the following steps:

[0010] (1) melt-blending and granulating PLA and CGA at a mass ratio of 100:1 to 100:15 to obtain PLA / CGA blended slices;

[0011] (2) melt spinning, drawing, and heat setting the PLA / CGA blended slices to obtain multifunctional PLA fibers; or, spunbonding the PLA / CGA blended slices to obtain multifunctional PLA nonwoven materials.

[0012] In one embodiment of the present invention, the PLA and CGA used in step (1) need to be dried before use so that the moisture content thereof is not higher than 300 ppm.

[0013] In one embodiment of the present invention, the content of dextrorotatory lactic acid structural unit D-LA in the PLA of step (1) is 0 to 10 mol%; or, a mixture of PLA with a D-LA content of 0 to 10 mol% and dextrorotatory polylactic acid PDLA, wherein the mass ratio of PLA to PDLA is 100:5 to 50:50.

[0014] In one embodiment of the present invention, the melt blending and granulation in step (1) is carried out using a twin-screw extruder, the granulation temperature is 150-230° C., and the screw speed is 300-500 rpm.

[0015] In one embodiment of the present invention, the melt blending and granulation in step (1) may be premixed in a high-speed mixer for 1 to 10 minutes.

[0016] In one embodiment of the present invention, the PLA / CGA blended chips prepared in step (1) need to be vacuum dried at 70-80° C. for 10-30 hours.

[0017] In one embodiment of the present invention, in the melt spinning of step (2), the spinning temperature is 180-240°C, the spinning speed is 1500-5000 m / min; the drawing temperature is 85-130°C, the drawing multiple is 4-10; and the heat setting temperature is 120-170°C.

[0018] In one embodiment of the present invention, the spunbond nonwoven processing of step (2) is specifically: spinning into a web and hot rolling reinforcement; wherein the spinning temperature is 180-240°C, the spinning speed is 3000-6000m / min, the web speed is 5-30m / min, and the pump supply is 30-150mL / min; the hot rolling line pressure is 65-75N / mm, and the roller temperature is 65-180°C.

[0019] The second object of the present invention is the multifunctional PLA fiber or multifunctional PLA nonwoven material prepared by the method of the present invention.

[0020] The third object of the present invention is to provide a functional textile, which uses the multifunctional PLA fiber or multifunctional PLA nonwoven material of the present invention.

[0021] In one embodiment of the present invention, the functional textile is obtained by weaving the multifunctional PLA fiber of the present invention or processing the multifunctional PLA nonwoven material.

[0022] The fourth object of the present invention is to use the multifunctional PLA fiber or multifunctional PLA nonwoven material of the present invention in the field of functional material preparation.

[0023] A fifth object of the present invention is to provide a method for increasing the content of chlorogenic acid in PLA textiles, comprising the following steps:

[0024] (1) melt-blending and granulating PLA and CGA at a mass ratio of 100:1 to 100:15 to obtain PLA / CGA blended slices;

[0025] (2) melt spinning, drawing, and heat setting the PLA / CGA blended slices to obtain multifunctional PLA fibers; or, spunbonding the PLA / CGA blended slices to obtain multifunctional PLA nonwoven materials.

[0026] A sixth object of the present invention is to provide a method for improving the oxidation resistance and UV resistance of PLA fibers, comprising the following steps:

[0027] (1) melt-blending and granulating PLA and CGA at a mass ratio of 100:1 to 100:15 to obtain PLA / CGA blended slices;

[0028] (2) The PLA / CGA blended chips are melt-spun, drawn, and heat-set to obtain antioxidant and UV-resistant PLA fibers.

[0029] [Beneficial Effects]

[0030] (1) The PLA resource used in the present invention is renewable and biodegradable, and using it as a raw material can solve the problems of resource shortage and environmental pollution in the development of synthetic fibers.

[0031] (2) Currently, the functionality of PLA fibers is low. The present invention uses natural extract CGA as a functional factor and introduces it into PLA to obtain PLA fibers and nonwoven materials with functions such as anti-oxidation and UV shielding, which can meet people's needs for functional PLA fibers and nonwoven materials.

[0032] (3) The natural extract CGA used in the present invention is derived from plants such as Eucommia ulmoides and honeysuckle. In addition to having antioxidant and UV shielding functions, it is harmless to the human body.

[0033] (4) The melting point of the natural extract CGA used in the present invention is about 210°C, which is close to the melting point of PLA, and is suitable for melt blending with PLA to prepare multifunctional PLA fibers and functional PLA nonwoven materials.

[0034] (5) The multifunctional PLA fiber and PLA nonwoven material prepared by the present invention can maintain the physical and mechanical properties of the PLA fiber itself and have good spinnability; at the same time, the introduction of CGA will not reduce the spinnability and mechanical properties of the PLA matrix, and can exert its anti-ultraviolet and anti-oxidation properties.

[0035] (6) The UV transmittance of the multifunctional PLA fiber prepared by the present invention is below 8%, the free radical scavenging rate is above 25.8%, and the strength is above 2.5 cN / dtex; the UV transmittance of the multifunctional PLA nonwoven material is below 2.6%, and the free radical scavenging rate is above 33.3%. DETAILED DESCRIPTION

[0036] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.

[0037] Test method:

[0038] 1. Test method for tensile mechanical properties:

[0039] The tensile mechanical properties of multifunctional polylactic acid fibers were tested in accordance with the national standard "GB / T 14344-2022 Test method for tensile properties of chemical fiber filaments".

[0040] 2. Antioxidant test method:

[0041] Weigh 3 mg of ABTS diammonium salt and 1 mg of K2S2O8 respectively, and dilute them with 0.735 mL and 1.43 mL of distilled water respectively. Mix the diluted solutions in a volume ratio of 1:1. After standing in a dark environment for 12 hours, dilute the mixed solution with PBS buffer until the absorbance at 734 nm is 0.70±0.02. This solution is the ABTS solution.

[0042] Take 1 mL of the prepared ABTS solution and add it to 5 mg of the sample. After leaving it at room temperature for 2 hours, measure the absorbance of the solution with an enzyme marker. Set up three groups of experiments for each sample, record the absorbance of the solution before and after the experiment, substitute the absorbance value into the following formula to calculate the ABTS free radical scavenging rate, and take the average value of the calculated results.

[0043]

[0044] Where: A splis the initial absorbance of ABTS solution; A ctrl Represents the absorbance of the ABTS solution 2 hours after adding the sample.

[0045] 3. UV shielding performance test method:

[0046] Fiber: Arrange the fibers tightly in parallel and stick both ends of the fibers on a rectangular mold (hollow in the middle, 3 cm long and 2.5 cm wide), with one layer on each side. Put the arranged fibers into the optical path of a UV-visible-near-infrared spectrophotometer to test their transmittance. The wavelength of UV-visible light is 200-600 nm, with an interval of 2 nm.

[0047] Nonwoven materials: Place the nonwoven material in the light path of a UV-visible-near infrared spectrophotometer to test its transmittance. The wavelength of UV-visible light is 200-600nm with an interval of 2nm.

[0048] Example 1

[0049] A method for preparing multifunctional PLA fiber containing chlorogenic acid comprises the following steps:

[0050] (1) Melt blending and granulation

[0051] PLA and CGA with a melt flow index of 8 g / 10 min (210° C., 2.16 kg) and a D-LA content of 0.25 mol% were dried in a vacuum oven at 75° C. for 24 h and set aside;

[0052] PLA and CGA were weighed in a mass ratio of 100:5 and put into a high-speed mixer for premixing for 5 minutes, and then melt-blended and granulated in a twin-screw blender at a granulation temperature of 190° C. and a screw speed of 400 rpm to obtain PLA / CGA blended slices; the obtained slices were vacuum dried at 75° C. for 24 hours for standby use;

[0053] (2) Preparation of multifunctional PLA fibers

[0054] The PLA / CGA blend slices were melt-spun (spinning temperature 195°C, spinning speed 2000m / min) to obtain primary multifilaments; then the primary multifilaments were stretched at a stretching temperature of 90°C and a stretching multiple of 6.0; finally, heat-set at a heat-setting temperature of 120°C to obtain multifunctional PLA multifilaments.

[0055] Comparative Example 1

[0056] The CGA in step (1) of Example 1 was omitted, and the other steps were the same as those of Example 1 to obtain PLA multifilament.

[0057] Comparative Example 2

[0058] When the mass ratio of PLA to CGA in step (1) of Example 1 is adjusted to 100:20 and the other conditions are kept the same as those of Example 1, it is difficult to prepare multifunctional PLA multifilament.

[0059] Comparative Example 3

[0060] It is difficult to prepare multifunctional PLA multifilament by adjusting the CGA in step (1) of Example 1 to tea polyphenols and keeping the other parts the same as Example 1.

[0061] The performance of the PLA multifilaments obtained in Example 1, Comparative Example 1 and Comparative Example 2 was tested, and the test results are as follows:

[0062] Table 1 Test results

[0063] example Strength (cN / dtex) UV transmittance (%) Free radical scavenging rate (%) Melting point(℃) Spinnability Example 1 2.8 5.6 26.7 171.2 good Comparative Example 1 3.0 60 / 173.0 good Comparative Example 2 / / / / Difference Comparative Example 3 / / / / Difference

[0064] It can be seen from Table 1 that the addition of 5% CGA does not affect the spinnability of PLA, but when 20% CGA is added, the spinnability of PLA is poor and it is difficult to spin continuously. That is, when a small amount of CGA is added, the spinnability will not be affected; while the addition of excessive CGA will affect the spinnability of PLA. In addition, when a small amount of CGA is added, the tensile mechanical properties of PLA fiber are not much different from those when no CGA is added. If CGA is adjusted to tea polyphenols, chemical reactions are likely to occur at high temperatures. During melt blending, PLA becomes black and brittle, making it difficult to spin.

[0065] Example 2

[0066] A method for preparing multifunctional PLA fiber containing chlorogenic acid comprises the following steps:

[0067] (1) Melt blending and granulation

[0068] PLA with a melt flow index of 8 g / 10 min (210° C., 2.16 kg) and a D-LA content of 0.25 mol%, dextrorotatory polylactic acid (PDLA) with a melt flow index of 16 g / 10 min (210° C., 2.16 kg), and CGA were dried in a vacuum oven at 75° C. for 24 h and set aside;

[0069] PLA, PDLA and CGA were weighed in a mass ratio of 50:50:5 and put into a high-speed mixer for premixing for 5 minutes, and then melt-blended and granulated in a twin-screw blender at a granulation temperature of 230° C. and a screw speed of 400 rpm to obtain stereocomposite PLA (sc-PLA) / CGA blended slices; the obtained slices were vacuum dried at 75° C. for 24 hours for use;

[0070] (2) Preparation of multifunctional PLA fibers

[0071] The sc-PLA / CGA blended slices were melt-spun (spinning temperature 235°C, spinning speed 2000m / min) to obtain primary multifilaments; then the primary multifilaments were stretched at a stretching temperature of 120°C and a stretching multiple of 6.0; finally, heat-set at a heat-setting temperature of 160°C to obtain multifunctional sc-PLA multifilaments.

[0072] The obtained multifunctional sc-PLA multifilament was subjected to performance testing, and the test results are as follows:

[0073] The strength is 3.2 cN / dtex, the UV transmittance is 7%, and the free radical scavenging rate is 25.8%.

[0074] Example 3

[0075] A method for preparing multifunctional PLA fiber containing chlorogenic acid comprises the following steps:

[0076] (1) Melt blending and granulation

[0077] PLA and CGA with a melt flow index of 8 g / 10 min (210° C., 2.16 kg) and a D-LA content of 0.25 mol% were dried in a vacuum oven at 75° C. for 24 h and set aside;

[0078] PLA and CGA were weighed in a mass ratio of 100:10 and put into a high-speed mixer for premixing for 5 minutes, and then melt-blended and granulated in a twin-screw blender at a granulation temperature of 190° C. and a screw speed of 400 rpm to obtain PLA / CGA blended slices; the obtained slices were vacuum dried at 75° C. for 24 hours for standby use;

[0079] (2) Preparation of multifunctional PLA fibers

[0080] The PLA / CGA blend slices were melt-spun (spinning temperature 195°C, spinning speed 2000m / min) to obtain primary multifilaments; then the primary multifilaments were stretched at a stretching temperature of 90°C and a stretching multiple of 6.0; finally, heat-set at a heat-setting temperature of 120°C to obtain multifunctional PLA multifilaments.

[0081] The obtained multifunctional PLA multifilament was subjected to performance test, and the test results are as follows:

[0082] The strength is 2.5 cN / dtex, the UV transmittance is 8%, and the free radical scavenging rate is 93.5%.

[0083] Example 4

[0084] A method for preparing a multifunctional PLA nonwoven material containing chlorogenic acid comprises the following steps:

[0085] (1) Melt blending and granulation

[0086] PLA and CGA with a melt flow index of 8 g / 10 min (210° C., 2.16 kg) and a D-LA content of 0.25 mol% were dried in a vacuum oven at 75° C. for 24 h and set aside;

[0087] PLA and CGA were weighed in a mass ratio of 100:5 and put into a high-speed mixer for premixing for 5 minutes, and then melt-blended and granulated in a twin-screw blender at a granulation temperature of 190° C. and a screw speed of 400 rpm to obtain PLA / CGA blended slices; the obtained slices were vacuum dried at 75° C. for 24 hours for standby use;

[0088] (2) Preparation of multifunctional PLA nonwoven materials

[0089] The PLA / CGA slices were used for spunbond nonwoven processing, and the multifunctional PLA spunbond nonwoven material was obtained by spinning (spinning temperature of 195°C, spinning speed of 3500m / min, web speed of 24m / min, pump supply of 48mL / min), hot rolling reinforcement (hot rolling line pressure of 70N / mm, hot rolling mill temperature of 70°C);

[0090] The obtained multifunctional PLA spunbonded nonwoven material was subjected to performance tests, and the test results are as follows:

[0091] Surface density: 35g / m 2 , UV transmittance is 2.6%, and free radical scavenging rate is 33.3%.

[0092] Example 5

[0093] A method for preparing a multifunctional PLA nonwoven material containing chlorogenic acid comprises the following steps:

[0094] (1) Melt blending and granulation

[0095] PLA and CGA with a melt flow index of 8 g / 10 min (210° C., 2.16 kg) and a D-LA content of 0.25 mol% were dried in a vacuum oven at 75° C. for 24 h and set aside;

[0096] Then, PLA and CGA were weighed in a mass ratio of 100:10 and put into a high-speed mixer for premixing for 5 minutes, and then melt-blended and granulated in a twin-screw blender at a granulation temperature of 190° C. and a screw speed of 400 rpm to obtain PLA / CGA blended slices; the obtained slices were vacuum dried at 75° C. for 24 hours for standby use;

[0097] (2) Preparation of multifunctional PLA nonwoven materials

[0098] The PLA / CGA slices were used for spunbond nonwoven processing, and the multifunctional PLA spunbond nonwoven material was obtained by spinning (spinning temperature of 195°C, spinning speed of 3500m / min, web speed of 24m / min, pump supply of 48mL / min), hot rolling reinforcement (hot rolling line pressure of 70N / mm, hot rolling mill temperature of 70°C);

[0099] The obtained multifunctional PLA spunbonded nonwoven material was subjected to performance tests, and the test results are as follows:

[0100] Surface density: 35g / m 2 , UV transmittance is 2.0%, and free radical scavenging rate is 96.8%.

[0101] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a multifunctional polylactic acid textile containing chlorogenic acid, characterized in that: The steps include: (1) melt-blending and granulating polylactic acid (PLA) and chlorogenic acid (CGA) in a mass ratio of 100:5 to 100:15 to obtain PLA / CGA blended slices; The melt blending granulation is carried out by a twin-screw extruder, the granulation temperature is 190°C, and the screw speed is 300-500rpm; the content of the right-lactic acid structural unit D-LA in PLA is 0-10mol%; (2) melt spinning, drawing, and heat setting the PLA / CGA blended slices to obtain multifunctional PLA fibers; or, spunbonding the PLA / CGA blended slices to obtain multifunctional PLA nonwoven materials; Among them, the spinning temperature in melt spinning is 195°C, the spinning speed is 1500~5000m / min; the drawing temperature is 85~130°C, the drawing multiple is 4~10; the heat setting temperature is 120~170°C; The specific processing of spunbond nonwovens is: spinning into a web and hot rolling reinforcement; the spinning temperature is 195°C, the spinning speed is 3000~6000m / min, the web speed is 5~30m / min, and the pump supply is 30~150mL / min; the hot rolling line pressure is 65~75N / mm, and the roller temperature is 65~70°C.

2. The multifunctional PLA fiber prepared by the method according to claim 1.

3. The multifunctional PLA nonwoven material prepared by the method described in claim 1.

4. A functional textile, characterized in that: The multifunctional PLA fiber described in claim 2 or the multifunctional PLA nonwoven material described in claim 3 is used.

5. Use of the multifunctional PLA fiber according to claim 2 or the multifunctional PLA nonwoven material according to claim 3 in the field of functional material preparation.

Citation Information

Patent Citations

  • Super-hydrophobic anti-ultraviolet flame-retardant silk fabric and preparation method thereof

    CN109736082A

  • Preparation method and application of polylactic acid / chitosan / honeysuckle chlorogenic acid nanofiber membrane

    CN113174702A

  • Manufacturing method of double-sided elastic interwoven antibacterial polar fleece cloth

    CN116815384A

  • Biological environment-friendly toughened strong antioxidant antibacterial polylactic acid composite material and preparation method thereof

    CN117126518A

  • Medical mask with a functional material

    US20130291878A1