A multi-component composite steel slag grinding aid activator and preparation method thereof

Through the use of multi-component composite steel slag grinding exciter, the use of zwitterionic polyacrylamide and other functional compounds to break the dense structure of iron and calcium minerals in steel slag, solving the problems of poor abrasion and low activity of steel slag grinding, significantly improving the Grinding effect and hydration activity.

CN117843276BActive Publication Date: 2024-11-26HUAXIN CEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311668139.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-07
Publication Date
2024-11-26
Estimated Expiration
2043-12-07

AI Technical Summary

Technical Problem

Steel slag has problems such as poor wearability and low activity during grinding. Traditional agitators are difficult to effectively play the role of grinding and activation, especially due to the high iron content in steel slag and the dense structure of C2S and C3S crystals, which lead to hydration. Low activity.

Method used

Using multi-component composite steel slag grinding excitants, including zwitterionic polyacrylamide, phenylthiocyanate/isothiocyanate compounds, benzene hydroxycarboxylic acid compounds, carbonic acid/bicarbonate compounds and thiocyanate compounds , through adsorption complexation, steric hindrance, charge repulsion and acid-base forces, the tight structure of iron and its compounds and calcium minerals in steel slag is broken, the surface energy is reduced, and chemical bond fracture and hydration reaction are promoted.

Benefits of technology

It significantly improves the grinding effect and hydration activity of steel slag, increases the specific surface area of ​​the powder surface, reduces the fineness, and improves the reactivity and strength of steel slag in cement concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004592288850000021
    Figure BDA0004592288850000021
  • Figure BDA0004592288850000101
    Figure BDA0004592288850000101
Patent Text Reader

Abstract

The invention discloses a multi-component composite steel slag grinding aid activator, which comprises the following components by mass percentage: 3-5% polyacrylamide polymer, 16-24% benzene hydroxycarboxylic acid compound, 8-15% benzene thiocyanate / isothiocyanate compound, 5-15% carbonic acid / bicarbonate compound, 5-15% thiocyanate compound, 0.5-1.0% penetrant, and the remainder is water. The invention aims at the mineral composition characteristics and chemical components of steel slag, effectively accelerates the breaking of chemical bonds inside the mineral material, reduces the surface energy of the powder, and thus achieves an excellent grinding aid effect. At the same time, the steel slag fineness is reduced, and the activity of the steel slag is stimulated by complexation and dissolution promotion, so that the steel slag has an obvious grinding aid stimulating effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of materials, and in particular relates to a multi-component composite steel slag grinding aid activator and a preparation method thereof. Background Art

[0002] Steel slag is waste slag produced by steelmaking, and its production volume is about 15-20% of crude steel production, and its annual production volume has exceeded 150 million tons. Although steel slag is widely used: used in metallurgical industry, used for wastewater treatment, used in agriculture, used in road engineering, etc., its comprehensive utilization rate is less than 30%. Steel slag not only has a large output, but also has a low utilization rate. Its accumulation in the natural environment will seriously occupy land resources and pollute the ecological environment. In recent years, the state has successively promulgated a number of laws and regulations to encourage the exploration of steel slag resource utilization. The mineral composition of steel slag is mainly RO phase, olivine, magnesium rhodonite, C2S, C3S, C4AF, C2F, which is similar to the mineral composition of cement clinker, so it is theoretically feasible for steel slag to replace cement clinker. Studies have shown that the specific surface area of ​​steel slag can be increased by pre-grinding steel slag, thereby significantly improving its activity. As the specific surface area of ​​steel slag increases, the activity of steel slag also increases. Adding grinding aids and activators during steel slag grinding can be used as an effective means to reduce grinding energy consumption and improve activity.

[0003] In the prior art, enhanced grinding aids based on polyols, polyol amines and inorganic salts have been widely used in cement. However, unlike cement clinker, the iron content in steel slag is much higher than that in cement clinker. Some iron and its compounds are closely embedded in the steel slag structure, and the presence of RO phase (iron-magnesium phase solid solution) in steel slag makes the steel slag difficult to grind. In the industrial steelmaking process, steel slag is formed in an extremely high temperature environment. The high temperature environment makes the structure of C2S and C3S crystals in the steel slag dense. At the same time, the grain size of the steel slag is large and has few defects. The extremely cold temperature process after the high temperature forms a large amount of glass inside the steel slag, and the presence of glass limits the hydration activity of the steel slag. Traditional cement grinding aids are difficult to play a good role in the grinding and activity stimulation of steel slag. It is very necessary to provide corresponding solutions to solve the problems of poor grindability and low activity according to the characteristics of steel slag.

[0004] CN 102503220B relates to a composite steel slag grinding aid, which solves the problems that the existing grinding aid is not suitable for steel slag grinding, has a long grinding time, low grinding efficiency, low early activity in the active utilization of steel slag, and a large content of particles not participating in the reaction. The technical scheme includes the following components in weight percentage: 15%-30% surfactant, 20%-40% grinding aid, 20-40% regulator, and 5-25% carrier. Its main components are polyol, triethanolamine, lignin sulfonic acid, etc., and the effect on steel slag is limited.

[0005] CN 104692706B discloses a grinding aid for vertical mill grinding steel slag, which is composed of the following raw materials in weight percentage: 1-5% polyacrylic acid, 5-10% molasses, 1-5% sodium hexametaphosphate, 2-6% ethylenediaminetetraacetic acid, 3-10% triethanolamine, 5-20% aluminum sulfate, and 46-81% carrier. The molecular weight of the acrylic acid used is 2000-5000. The polyacrylic acid has poor thermal stability and a molecular weight of 2000-5000, and it is difficult to work after pyrolysis. Ethylenediaminetetraacetic acid, triethanolamine and aluminum sulfate are coordinated as steel slag quality modifiers to improve the reaction activity of steel slag in cement concrete. Ethylenediaminetetraacetic acid has a great influence on the reaction of Ca 2+ Mg 2+ , Fe 3+ , Fe 2+ All metal ions have a certain chelating effect. When water is added to steel slag powder and cement, the concentration of metal ions can be effectively reduced, which is conducive to the dissolution of more metal ions and promotes the reaction activity of the cementitious system. However, its chelating effect on the iron present in large quantities in steel slag is limited.

[0006] The above disclosed patented technologies mainly use the currently commonly used grinding aids, such as alcohol amines, polyols, and inorganic salts, as the raw material system, and compound some functional components, which have limited effect on stimulating the grinding of steel slag. Summary of the invention

[0007] The purpose of the present invention is to provide a multi-component composite steel slag grinding aid activator and a preparation method thereof, which can effectively accelerate the breaking of chemical bonds inside mineral materials and reduce the surface energy of powders according to the mineral composition characteristics and chemical components of steel slag, thereby achieving excellent grinding aid effect; at the same time, by reducing the fineness of steel slag and stimulating the activity of steel slag through complexation and dissolution, it has a significant grinding aid stimulating effect on steel slag.

[0008] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0009] A multi-component composite steel slag grinding aid activator, the composition is calculated by mass percentage as follows:

[0010]

[0011] The rest is water.

[0012] According to the above scheme, the polyacrylamide polymer is zwitterionic polyacrylamide with a molecular weight range of 300,000 to 500,000 g / mol.

[0013] According to the above scheme, the structure of the benzene-containing hydroxycarboxylic acid compound is that at least one carboxyl group, carboxymethyl group or carboxyethyl group is grafted onto the benzene ring, and at the same time at least one hydroxyl group or hydroxymethyl group is grafted onto the benzene ring.

[0014] According to the above scheme, the benzene-containing hydroxycarboxylic acid compound is 2-hydroxybenzoic acid, m-hydroxybenzoic acid, 2-(hydroxymethyl)benzoic acid, 3-hydroxymethylbenzoic acid, 4-hydroxymethylbenzoic acid, p-hydroxymethylbenzoic acid, 2,3-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,3,4-trihydroxybenzoic acid, 2,4,5-trihydroxybenzoic acid, One or any mixture of hydroxybenzoic acid, 2,4,6-trihydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid, o-hydroxyphenylacetic acid, 3-hydroxyphenylacetic acid, 4-(hydroxymethyl)phenylacetic acid, p-hydroxyphenylacetic acid, 2,4-dihydroxyphenylacetic acid, 3,4-dihydroxyphenylacetic acid, 3,5-dihydroxyphenylacetic acid, p-hydroxyphenylpropionic acid, 3-(2-hydroxyphenyl)propionic acid, 3,4-dihydroxyphenylpropionic acid, 3,5-dihydroxyphenylpropionic acid.

[0015] According to the above scheme, the structure of the phenylthiocyanate / isothiocyanate compound is that at least one group containing N≡CS- or S=C=N-functional group is grafted onto the benzene ring.

[0016] According to the above scheme, the phenylthiocyanate / isothiocyanate-containing compound is one of benzyl thiocyanate, phenyl thioisocyanate, benzyl isothiocyanate, o-toluene isothiocyanate, m-toluene isothiocyanate, p-phenylene diisothiocyanate, 2-phenylethyl isothiocyanate, 4-methoxyphenyl isothiocyanate, benzoyl isothiocyanate, 3-carboxyl phenyl isothiocyanate, 3-chlorophenyl isothiocyanate, 4-bromophenyl isothiocyanate, and 4-iodophenyl isothiocyanate, or any mixture thereof.

[0017] According to the above scheme, the carbonate / bicarbonate compound is one of potassium carbonate, sodium carbonate, potassium bicarbonate, sodium bicarbonate or any mixture thereof.

[0018] According to the above scheme, the thiocyanate compound is one of sodium thiocyanate and potassium thiocyanate or any mixture thereof.

[0019] According to the above scheme, the penetrant is one of tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxypropylene stearate, polyoxyethylene lanolin ether, sorbitan laurate, polyoxyethylene polyoxypropylene oleate or any mixture thereof.

[0020] The preparation method of the multi-component composite steel slag grinding aid activator comprises the following steps:

[0021] Heat water, polyacrylamide polymer and penetrant to 30-50°C and maintain under stirring condition of 200-300 r / min;

[0022] Add the carbonic acid / bicarbonate compound and the thiocyanate compound and continue stirring for 15 to 30 minutes;

[0023] The benzene hydroxycarboxylic acid compound and the benzene thiocyanate / isothiocyanate compound are slowly added under stirring at 300-400 r / min, and stirring is continued for 20-30 minutes to obtain the multi-component composite steel slag grinding aid activator.

[0024] In the present invention, the zwitterionic polyacrylamide is a stable carrier of the grinding aid system, and other organic and inorganic components are evenly dispersed in the system through chain segment entanglement and hydrogen bonding, thereby promoting the effects of other components. On the other hand, the charge properties of the zwitterionic polyacrylamide effectively shield the positive and negative charges generated by the breakage of chemical bonds inside the steel slag mineral, and the macromolecular chain segments prevent the particles from approaching each other. At the same time, the oxygen and nitrogen atoms in the polyacrylamide and the Fe in the steel slag are 3+ 、Al 3+ Selective bonding significantly reduces its surface energy, thus playing a good grinding aid effect. Select a zwitterionic polyacrylamide polymer with a molecular weight of 300,000 to 500,000 g / mol. If the molecular weight is too small, it cannot effectively play a uniform dispersion role. If the molecular weight is too large, excessive entanglement and wrapping are not conducive to the effect of other components.

[0025] The N≡CS- or S=C=N- functional groups in the structure of phenylthiocyanate / isothiocyanate compounds can selectively bond with different forms of iron in steel slag, reduce the surface energy of iron-containing minerals in steel slag, induce the migration of the surface lattice position of iron-containing minerals, generate point or line defects, break the tightly embedded structure formed by iron and its compounds and steel slag, and weaken the strength and hardness of the structure. The benzene ring in the structure of phenylthiocyanate / isothiocyanate compounds has greater steric hindrance than the short carbon chain of polyols and polyol amines. The N≡CS- or S=C=N- functional groups are adsorbed on the inner wall of the cracks of iron-containing minerals and further enter the depths of the cracks. With the formation and continuous expansion of the cracks, they play a "wedge" role, not only preventing the cracks from closing, but also promoting the crack expansion and accelerating the crack width. Thus, they have an excellent grinding aid effect on iron and its compounds in steel slag.

[0026] The hydroxyl and carboxyl functional groups in the structure of benzene-containing hydroxycarboxylic acid compounds can selectively bond with calcium in steel slag, reduce the surface energy of calcium-containing minerals in steel slag, induce the migration of the surface lattice position of calcium-containing minerals, generate point or line defects, break the dense structure of C2S and C3S crystals of calcium-containing minerals in steel slag, and weaken the strength and hardness of the structure. The benzene ring in the structure of benzene-containing hydroxycarboxylic acid compounds has greater steric hindrance than the short carbon chain of polyols and polyol amines. The hydroxyl and carboxyl functional groups are adsorbed on the inner wall of the cracks of calcium-containing minerals and further enter the depth of the cracks. With the formation and continuous expansion of the cracks, they play a "wedge" role, not only preventing the cracks from closing, but also promoting the crack expansion and accelerating the crack width. Therefore, it has an excellent grinding aid effect on calcium and its compounds in steel slag.

[0027] Penetrants with appropriate surface tension can effectively reduce the surface tension of the system, promote the wetting and penetration of phenylthiocyanate / isothiocyanate compounds and benzene hydroxycarboxylic acid compounds on the surface of steel slag minerals, and make them play a better grinding aid role. Further, penetrants containing oxygen atoms are selected, and the oxygen atoms in their structure can bond with the metal oxides after the steel slag minerals are ground, thus playing a grinding aid role.

[0028] During the grinding process, carbonate / bicarbonate compounds and thiocyanate compounds react with Ca on the surface of the slag mineral phase through acid-base interaction. 2+ Mg 2+ 、Al 3+ and Fe 3+ The complexation reaction leads to a significant increase in polar surface energy and alkalinity constant. The electrical repulsion between particles prevents them from approaching and agglomerating with each other. In addition, free Na + , K + will enter the lattice holes or interact with Ca in the lattice 2+ Mg 2+ 、Al 3+ and Fe 3+ Substitution occurs, further aggravating the mineral lattice distortion and accelerating the breaking of chemical bonds inside the slag.

[0029] Steel slag has a high C2S content, but it has low hydration activity in the early stage, but has high carbonization activity. The carbonate / bicarbonate in the carbonate / bicarbonate compound can accelerate the dissolution of C2S ions in water and promote the dissolved calcium and silicon to participate in hydration. Steel slag has a high iron content, and the thiocyanate in the thiocyanate compound has a selective complexing effect on iron, which promotes the dissolution of iron ions and allows more iron ions to participate in hydration. The main C2S minerals and iron solid-solution minerals in the steel slag effectively participate in the hydration reaction of the cement system, stimulating the activity of the steel slag.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. According to the characteristics of the mineral composition of steel slag, starting from the structure of organic matter and the characteristics of inorganic salts, organic phenylthiocyanate / isothiocyanate compounds, benzene hydroxycarboxylic acid compounds and inorganic carbonate / bicarbonate compounds, thiocyanate compounds are used to cooperate with each other through adsorption complexation, steric hindrance, charge repulsion, acid-base interaction, etc., which have a significant grinding-aiding effect on the tight embedded structure formed by the difficult-to-grind iron and its compounds in the steel slag and the dense structure of the calcium-containing minerals C2S and C3S crystals in the steel slag.

[0032] 2. Selecting an oxygen-containing penetrant with appropriate surface tension can not only play a grinding aid role, but also effectively reduce the surface tension of the system, promote the wetting and penetration of phenylthiocyanate / isothiocyanate compounds and benzene hydroxycarboxylic acid compounds on the surface of steel slag minerals, and further promote the grinding aid effect.

[0033] 3. Select zwitterionic polyacrylamide with appropriate molecular weight to effectively stabilize the system, promote its dispersion, and at the same time have a good grinding aid effect.

[0034] 4. In view of the difficult-to-hydrate mineral chemical composition in steel slag, carbonate / bicarbonate can accelerate the dissolution of C2S ions in water, and thiocyanate can promote the dissolution of iron ions. Combined with the grinding aid effect to improve the fineness of steel slag, the activity of steel slag can be effectively stimulated. DETAILED DESCRIPTION

[0035] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention. The following specific examples are only some preferred embodiments of the present invention, rather than all embodiments. Based on the embodiments of the present invention, modifications, substitutions and improvements made by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0036] The specific implementation method provides a multi-component composite steel slag grinding aid activator, the components of which are calculated by mass percentage as follows: 3-5% polyacrylamide polymer, 16-24% benzene hydroxycarboxylic acid compound, 8-15% benzene thiocyanate / isothiocyanate compound, 5-15% carbonic acid / bicarbonate compound, 5-15% thiocyanate compound, 0.5-1.0% penetrant, and the rest is water.

[0037] Specifically, the polyacrylamide polymer is zwitterionic polyacrylamide with a molecular weight ranging from 300,000 to 500,000 g / mol.

[0038] Specifically, the structure of the benzene-containing hydroxycarboxylic acid compound is that at least one carboxyl group, carboxymethyl group or carboxyethyl group is grafted onto the benzene ring, and at least one hydroxyl group or hydroxymethyl group is grafted onto the benzene ring.

[0039] Specifically, the benzene-containing hydroxycarboxylic acid compound is 2-hydroxybenzoic acid, m-hydroxybenzoic acid, 2-(hydroxymethyl)benzoic acid, 3-hydroxymethylbenzoic acid, 4-hydroxymethylbenzoic acid, p-hydroxymethylbenzoic acid, 2,3-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,3,4-trihydroxybenzoic acid, 2,4,5-trihydroxybenzoic acid, The invention can be any one of the following: 2,4,6-trihydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid, o-hydroxyphenylacetic acid, 3-hydroxyphenylacetic acid, 4-(hydroxymethyl)phenylacetic acid, p-hydroxyphenylacetic acid, 2,4-dihydroxyphenylacetic acid, 3,4-dihydroxyphenylacetic acid, 3,5-dihydroxyphenylacetic acid, p-hydroxyphenylpropionic acid, 3-(2-hydroxyphenyl)propionic acid, 3,4-dihydroxyphenylpropionic acid, and 3,5-dihydroxyphenylpropionic acid, or any mixture thereof.

[0040] Specifically, the structure of the phenylthiocyanate / isothiocyanate compound is that at least one group containing a N≡CS- or S=C=N-functional group is grafted onto a benzene ring.

[0041] Specifically, the phenylthiocyanate / isothiocyanate compound is one of benzyl thiocyanate, phenyl thioisocyanate, benzyl isothiocyanate, o-toluene isothiocyanate, m-toluene isothiocyanate, p-phenylene diisothiocyanate, 2-phenylethyl isothiocyanate, 4-methoxyphenyl isothiocyanate, benzoyl isothiocyanate, 3-carboxylphenyl isothiocyanate, 3-chlorophenyl isothiocyanate, 4-bromophenyl isothiocyanate, and 4-iodophenyl isothiocyanate, or any mixture thereof.

[0042] Specifically, the carbonate / bicarbonate compound is one of potassium carbonate, sodium carbonate, potassium bicarbonate, sodium bicarbonate, or any mixture thereof.

[0043] Specifically, the thiocyanate compound is one of sodium thiocyanate and potassium thiocyanate or any mixture thereof.

[0044] Specifically, the penetrant is one of tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxypropylene stearate, polyoxyethylene lanolin ether, sorbitan laurate, polyoxyethylene polyoxypropylene oleate, or any mixture thereof.

[0045] The specific implementation also provides a method for preparing the above-mentioned multi-component composite steel slag grinding aid activator, comprising the following steps:

[0046] Water, polyacrylamide polymer and penetrant are added to a container in sequence, heated to 30-50°C and maintained at 200-300 r / min while stirring, and then a carbonate / bicarbonate compound and a thiocyanate compound are added while stirring to fully dissolve them. After stirring for 15-30 minutes, a benzene hydroxycarboxylic acid compound and a benzene thiocyanate / isothiocyanate compound are slowly added at 300-400 r / min, and stirring is continued for 20-30 minutes to obtain the multi-component composite steel slag grinding aid activator.

[0047] Example 1

[0048] 62.5g of water, 3.0g of zwitterionic polyacrylamide with a molecular weight of 300000g / mol, and 0.5g of tetraethylene glycol monostearate are added to a container in sequence, heated to 30°C and maintained under stirring at 200r / min, and then 5.0g of potassium carbonate and 5.0g of sodium thiocyanate are added under stirring to fully dissolve them. After stirring for 15min, 16.0g of 2-hydroxybenzoic acid and 8.0g of benzyl thiocyanate are slowly added under 300r / min, and stirring is continued for 20min to obtain the multi-component composite steel slag grinding aid activator.

[0049] Example 2

[0050] 25.0g of water, 5.0g of zwitterionic polyacrylamide with a molecular weight of 500000g / mol, and 1.0g of tetraethylene glycol monooleate are added to a container in sequence, heated to 50°C and maintained at 300r / min while stirring, and then 15.0g of sodium carbonate and 15.0g of potassium thiocyanate are added while stirring to fully dissolve them. After stirring for 30min, 24.0g of 4-hydroxymethylbenzoic acid and 15.0g of benzyl thiocyanate are slowly added at 400r / min, and stirring is continued for 30min to obtain the multi-component composite steel slag grinding aid activator.

[0051] Example 3

[0052] 44.6g of water, 3.4g of zwitterionic polyacrylamide with a molecular weight of 400000g / mol, and 0.8g of polyoxypropylene mannitol dioleate are added to a container in sequence, heated to 40°C and maintained under the condition of 245r / min while stirring, and then 15.0g of potassium bicarbonate and 5.0g of potassium thiocyanate are added under stirring to fully dissolve them. After stirring for 25min, 18.7g of 2,4-dihydroxybenzoic acid and 12.5g of o-toluene isothiocyanate are slowly added under the condition of 340r / min, and stirring is continued for 21min to obtain the multi-component composite steel slag grinding aid activator.

[0053] Example 4

[0054] 43.5 g of water, 4.3 g of zwitterionic polyacrylamide with a molecular weight of 350,000 g / mol, and 0.6 g of polyoxypropylene stearate are added to a container in sequence, heated to 32° C. and maintained at 289 r / min while stirring, and then 5.0 g of sodium bicarbonate and 15.0 g of sodium thiocyanate are added while stirring to fully dissolve them. After stirring for 24 minutes, 19.8 g of 3,5-dihydroxybenzoic acid and 11.8 g of 2-phenylethyl isothiocyanate are slowly added at 360 r / min, and stirring is continued for 29 minutes to obtain the multi-component composite steel slag grinding aid activator.

[0055] Example 5

[0056] 45.8g of water, 4.8g of zwitterionic polyacrylamide with a molecular weight of 450000g / mol, and 0.7g of polyoxyethylene lanolin alcohol ether are added to a container in sequence, heated to 48°C and maintained under stirring at 242r / min, and then 9.8g of potassium carbonate and 7.3g of potassium thiocyanate are added under stirring to fully dissolve them. After stirring for 16min, 22.3g of 2,4,5-trihydroxybenzoic acid and 9.3g of 4-methoxyphenyl isothiocyanate are slowly added under 346r / min, and stirring is continued for 28min to obtain the multi-component composite steel slag grinding aid activator.

[0057] Example 6

[0058] 50.0g of water, 4.6g of zwitterionic polyacrylamide with a molecular weight of 300000g / mol, and 0.6g of anhydrous sorbitan laurate are added to a container in sequence, and heated to 43°C and maintained under the condition of 213r / min while stirring, and then 6.4g of sodium carbonate and 6.4g of sodium thiocyanate are added under stirring to fully dissolve them. After stirring for 18min, 23.5g of 5-hydroxyisophthalic acid and 8.5g of benzoyl isothiocyanate are slowly added under the condition of 313r / min, and stirring is continued for 23min to obtain the multi-component composite steel slag grinding aid activator.

[0059] Example 7

[0060] 52.8g of water, 3.1g of zwitterionic polyacrylamide with a molecular weight of 500000g / mol, and 0.9g of polyoxyethylene polyoxypropylene oleate are added to a container in sequence, heated to 37°C and maintained under the condition of 253r / min while stirring, and then 7.8g of potassium bicarbonate and 9.8g of sodium thiocyanate are added under stirring to fully dissolve them. After stirring for 23min, 17.3g of p-hydroxyphenylacetic acid and 8.3g of 3-carboxyl isothiocyanate are slowly added under the condition of 389r / min, and stirring is continued for 22min to obtain the multi-component composite steel slag grinding aid activator.

[0061] Example 8

[0062] 44.1g of water, 3.3g of zwitterionic polyacrylamide with a molecular weight of 400000g / mol, and 0.5g of polyoxyethylene polyoxypropylene oleate are added to a container in sequence, and heated to 35°C and maintained at 238r / min while stirring, and then 14.3g of sodium bicarbonate and 6.8g of potassium thiocyanate are added while stirring to fully dissolve them. After stirring for 29min, 16.7g of 3,4-dihydroxyphenylacetic acid and 14.3g of 3-chloroisothiocyanate are slowly added at 373r / min, and stirring is continued for 27min to obtain the multi-component composite steel slag grinding aid activator.

[0063] Example 9

[0064] 34.1g of water, 4.5g of zwitterionic polyacrylamide with a molecular weight of 450000g / mol, and 1.0g of anhydrous sorbitan laurate are added to a container in sequence, heated to 36°C and maintained under the condition of 276r / min while stirring, and then 13.8g of sodium carbonate and 14.3g of potassium thiocyanate are added under stirring to fully dissolve them. After stirring for 27min, 18.8g of 3,4-dihydroxyphenylpropionic acid and 13.5g of 4-iodoisothiocyanate are slowly added under the condition of 352r / min, and stirring is continued for 26min to obtain the multi-component composite steel slag grinding aid activator.

[0065] Example 10

[0066] 35.6g water, 1.9g zwitterionic polyacrylamide with a molecular weight of 350000g / mol, 2.0g zwitterionic polyacrylamide with a molecular weight of 500000g / mol, 0.2g tetraethylene glycol monostearate, 0.3g polyoxypropylene stearate, and 0.3g polyoxyethylene lanolin alcohol ether were added to the container in sequence, and heated to 42°C and maintained at 289r / min while stirring, and then 6.1g sodium carbonate, 6.1g sodium carbonate, and 1.2g sodium carbonate were added to the container in a stirring manner. g potassium bicarbonate, 5.3 g sodium thiocyanate, and 9.1 g potassium thiocyanate were fully dissolved, and after stirring for 28 min, 10.2 g p-hydroxymethylbenzoic acid, 5.3 g 3-hydroxyphenylacetic acid, 5.0 g 3-(2-hydroxyphenyl)propionic acid, 1.6 g benzyl thiocyanate, 5.4 g phenyl thioisocyanate, and 5.6 g p-phenylene diisothiocyanate were slowly added at 335 r / min, and stirring was continued for 25 min to obtain the multi-component composite steel slag grinding aid activator.

[0067] Comparative Example 1

[0068] Example 1 was repeated, except that an equal amount of zwitterionic polyacrylamide was replaced by polyallylamine, and other conditions remained unchanged, to obtain comparative sample 1.

[0069] Comparative Example 2

[0070] Example 1 was repeated, except that an equal amount of zwitterionic polyacrylamide was replaced by polyacrylic acid, and other conditions remained unchanged, to obtain comparative sample 2.

[0071] Comparative Example 3

[0072] Example 3 was repeated, except that an equal amount of polyoxypropylene mannitol dioleate was replaced by water while keeping other conditions unchanged, to obtain comparative sample 3.

[0073] Comparative Example 4

[0074] Example 4 was repeated, except that an equal amount of sodium bicarbonate was replaced by sodium sulfate, and an equal amount of sodium thiocyanate was replaced by sodium chloride, and other conditions remained unchanged, to obtain comparative sample 4.

[0075] Comparative Example 5

[0076] Example 5 was repeated, except that an equal amount of 2,4,5-trihydroxybenzoic acid was replaced by triethanolamine, an equal amount of 4-methoxyphenyl isothiocyanate was replaced by diethylene glycol, and other conditions remained unchanged, to obtain comparative sample 5.

[0077] The multi-component composite steel slag grinding aid activator prepared in the above Examples 1 to 10, the comparative samples prepared in Comparative Examples 1 to 5, a commercially available cement grinding aid, and a blank group without grinding aid were tested and evaluated.

[0078] Take 5kg of steel slag and add it to the test small mill. Before grinding, add the grinding aid evenly to the surface of the steel slag three times. The grinding aid dosage is 0.10%, and the grinding time is fixed for 30min. The grinding aid effect and performance are evaluated and tested. The steel slag used has a CaO content of 40.54%, a SiO2 content of 12.99%, and a Fe2O3 content of 19.44%. The main mineral phases are C2S and calcium iron aluminum stone. Among them, the grinding aid effect is evaluated by specific surface area and fineness sieve residue; the strength activity of steel slag powder is tested by replacing PO 42.5 cement with 30% mass. The specific surface area test refers to GB / T 8074-2008 "Blaine method for determination of specific surface area of ​​cement". The fineness test refers to GB / T 1345-2005 "Sieve analysis method for testing cement fineness". The strength test refers to GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)".

[0079] Table 1 Fineness index test of steel slag samples out of the mill

[0080] serial number <![CDATA[Specific surface area / m 2 / kg]]> 80μm sieve residue / % 45μm sieve residue / % Blank group 325.7 3.5 19.8 Commercial cement grinding aids 330.5 2.9 18.9 Comparative Example 1 335.6 2.8 18.2 Comparative Example 2 338.5 2.8 18.0 Comparative Example 3 349.5 2.6 17.2 Comparative Example 4 330.8 2.7 17.0 Comparative Example 5 340.3 2.8 18.1 Example 1 376.3 1.9 14.2 Example 2 369.5 2.0 15.3 Example 3 378.5 2.1 14.9 Example 4 370.6 1.8 14.0 Example 5 378.6 2.0 15.2 Example 6 375.0 1.6 15.0 Example 7 369.9 1.5 14.6 Example 8 375.6 2.0 14.3 Example 9 377.3 1.7 14.8 Example 10 374.5 1.8 14.6

[0081] As can be seen from Table 1, compared with the blank group, the multi-component composite steel slag grinding aid activator prepared in this patent has a larger specific surface area of ​​the ground steel slag powder and a lower sieve residue after grinding, and has a significant grinding aid effect. It is significantly better than the commercially available cement grinding aid and the sample effects obtained in Comparative Examples 1 to 5, indicating that the substances used in this patent can synergize with each other to exert a grinding aid effect, and it is difficult to achieve the same grinding aid effect by removing one component or replacing it with other components.

[0082] Table 2 Strength test of steel slag samples out of the mill

[0083]

[0084] As can be seen from Table 2, compared with the blank group, the multi-component composite steel slag grinding aid activator prepared by this patent has higher flexural strength and compressive strength at all ages of the ground steel slag powder, has obvious strength stimulating effect, and is significantly better than the commercially available cement grinding aid and the samples obtained in Comparative Examples 1 to 5, indicating that the substances used in this patent can synergize with each other to exert stimulating effects, and it is difficult to achieve the same stimulating effect by removing one component or replacing it with other components.

Claims

1. A multi-component composite steel slag grinding aid activator, characterized in that The composition is calculated by mass percentage as follows: Polyacrylamide polymer 3~5%, Contains 16-24% benzene hydroxycarboxylic acid compounds, Contains phenylthiocyanate / isothiocyanate compounds 8~15%, Carbonic acid / bicarbonate compounds 5~15%, Thiocyanate compounds 5~15%, Penetrant 0.5~1.0%, The rest is water; Wherein, the polyacrylamide polymer is zwitterionic polyacrylamide with a molecular weight range of 300000-500000 g / mol.

2. The multi-component composite steel slag grinding aid activator as claimed in claim 1, characterized in that The structure of the benzene-containing hydroxycarboxylic acid compound is that at least one carboxyl group, carboxymethyl group or carboxyethyl group is grafted onto the benzene ring, and at the same time at least one hydroxyl group or hydroxymethyl group is grafted onto the benzene ring.

3. The multi-component composite steel slag grinding aid activator as claimed in claim 2, characterized in that The benzene-containing hydroxycarboxylic acid compound is 2-hydroxybenzoic acid, m-hydroxybenzoic acid, 2-(hydroxymethyl)benzoic acid, 3-hydroxymethylbenzoic acid, 4-hydroxymethylbenzoic acid, p-hydroxymethylbenzoic acid, 2,3-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,3,4-trihydroxybenzoic acid, 2,4,5-trihydroxybenzoic acid. Formic acid, 2,4,6-trihydroxybenzoic acid, 4-hydroxyphthalic acid, 5-hydroxyisophthalic acid, o-hydroxyphenylacetic acid, 3-hydroxyphenylacetic acid, 4-(hydroxymethyl)phenylacetic acid, p-hydroxyphenylacetic acid, 2,4-dihydroxyphenylacetic acid, 3,4-dihydroxyphenylacetic acid, 3,5-dihydroxyphenylacetic acid, p-hydroxyphenylpropionic acid, 3-(2-hydroxyphenyl)propionic acid, 3,4-dihydroxyphenylpropionic acid, 3,5-dihydroxyphenylpropionic acid or any mixture thereof.

4. The multi-component composite steel slag grinding aid activator as claimed in claim 1, characterized in that The structure of the phenylthiocyanate / isothiocyanate compound is that at least one group containing a N≡C−S− or S=C=N− functional group is grafted onto a benzene ring.

5. The multi-component composite steel slag grinding aid activator as claimed in claim 4, characterized in that The phenylthiocyanate / isothiocyanate-containing compound is one of benzyl thiocyanate, phenyl thioisocyanate, benzyl isothiocyanate, o-toluene isothiocyanate, m-toluene isothiocyanate, p-phenylene diisothiocyanate, 2-phenylethyl isothiocyanate, 4-methoxyphenyl isothiocyanate, benzoyl isothiocyanate, 3-carboxyl phenyl isothiocyanate, 3-chlorophenyl isothiocyanate, 4-bromophenyl isothiocyanate, and 4-iodophenyl isothiocyanate, or any mixture thereof.

6. The multi-component composite steel slag grinding aid activator as claimed in claim 1, characterized in that The carbonate / bicarbonate compound is one of potassium carbonate, sodium carbonate, potassium bicarbonate, sodium bicarbonate or any mixture thereof.

7. The multi-component composite steel slag grinding aid activator as claimed in claim 1, characterized in that The thiocyanate compound is one of sodium thiocyanate and potassium thiocyanate or any mixture thereof.

8. The multi-component composite steel slag grinding aid activator as claimed in claim 1, characterized in that The penetrant is one of tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxypropylene stearate, polyoxyethylene lanolin ether, sorbitan laurate, polyoxyethylene polyoxypropylene oleate or any mixture thereof.

9. The method for preparing the multi-component composite steel slag grinding aid activator according to claim 1, characterized in that The following steps are involved: Heat water, polyacrylamide polymer and penetrant to 30-50°C and maintain under stirring condition of 200-300 r / min; Add the carbonic acid / bicarbonate compound and the thiocyanate compound and continue stirring for 15 to 30 minutes; The benzene hydroxycarboxylic acid compound and the benzene thiocyanate / isothiocyanate compound are slowly added under stirring at 300-400 r / min, and stirring is continued for 20-30 min to obtain the multi-component composite steel slag grinding aid activator.