A green and environmentally friendly ceramic glaze and preparation method thereof

A ceramic glaze formulation with attapulgite, bentonite, zircon, and other additives improves mechanical properties and wear resistance, addressing the limitations of existing glazes.

CN117865481BActive Publication Date: 2024-12-06ZIBO JINDING GLAZE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410045880.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2024-12-06
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

Existing ceramic glazes lack mechanical properties and wear resistance, necessitating the development of a new, environmentally friendly formulation.

Method used

A ceramic glaze comprising attapulgite, bentonite, zircon, quartz, calcium feldspar, pyrolusite, molybdenum oxide, melamine, and polyvinyl alcohol, with specific particle sizes and preparation methods to enhance mechanical properties and wear resistance.

Benefits of technology

The glaze exhibits improved mechanical properties and wear resistance through the synergistic effects of quartz and calcium feldspar, pyrolusite and MoO3, and melamine's high-temperature aluminum nitride production, resulting in enhanced glaze layer performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the field of ceramic technology, and specifically relates to a green and environmentally friendly ceramic glaze and a preparation method thereof. The glaze comprises the following components in parts by weight: 50-70 parts of attapulgite; 20-40 parts of bentonite; 10-30 parts of zircon; 5-15 parts of quartz; 4-10 parts of calcium feldspar; 3-5 parts of pyrolusite; 2-6 parts of molybdenum oxide; 4-8 parts of melamine; 1-3 parts of polyvinyl alcohol 2000; and 40-60 parts of water. The mechanical properties of the glaze layer can be improved by adding quartz and calcium feldspar, while calcium feldspar affects the stability of zircon production of ZrO2; the mechanical properties are further improved by adding pyrolusite and MoO3 composite to catalyze the production of mullite, and the added melamine can produce aluminum nitride with aluminum under high temperature conditions, thereby improving the mechanical properties and wear resistance of the glaze layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of ceramic technology, and more specifically, relates to a green and environmentally friendly ceramic glaze and a preparation method thereof. Background Art

[0002] Ceramic glaze is an indispensable raw material in the production process of ceramic tiles. It has the functions of covering and decoration. According to its different uses, it is mainly divided into surface glaze, polished glaze, matte glaze and dry granular glaze. Ceramic glaze can give ceramics certain mechanical properties and wear resistance.

[0003] CN116789364A discloses a wear-resistant glaze and a preparation method thereof, which relates to the field of ceramic glazes, including a surface glaze layer and a full-polished glaze layer. The surface glaze layer is made of the following raw materials in parts by weight: potassium feldspar: 20-40 parts; sodium feldspar: 25-35 parts; kaolin: 5-15 parts; calcined kaolin: 5-15 parts; calcined alumina: 20-25 parts; dolomite: 1-5 parts; nepheline: 2-8 parts; quartz : 2-6 parts; the full polishing glaze layer is made of the following raw materials by weight: albite: 50-60 parts; kaolin: 5-15 parts; calcined kaolin: 2-7 parts; calcined alumina: 1-3 parts; dolomite: 10-20 parts; quartz: 0.5-1.5 parts; calcined zinc oxide: 2-6 parts; strontium carbonate: 2-10 parts; calcined talc: 1-5 parts; wollastonite: 1-5 parts; corundum 0.5-1.5 parts. The application has the effect of improving the wear resistance of ceramic tiles.

[0004] CN116854371A discloses a high-strength wear-resistant glaze and a method for preparing high-strength ceramics using the same, belonging to the field of ceramic technology. The high-strength wear-resistant glaze of the present invention comprises the following components: 6 to 9 parts of kaolin, silicon dioxide, zirconium oxide, potassium feldspar, sodium feldspar, barium oxide, sodium oxide, praseodymium oxide, aegirine, amphibole, aragonite and vermiculite. When the obtained high-strength ceramic glaze is used to produce ceramic products, the production process is simple, suitable for mass production, and reduces the production cost of the enterprise.

[0005] CN116986819A discloses a corrosion-resistant ceramic glaze and a preparation method thereof, and relates to the technical field of production of ceramic glazes. The glaze is prepared from the following raw material components: feldspar, kaolin, refractory clay, zirconium silicate, zirconium oxide, zircon, graphene oxide, calcium oxide and deionized water; the feldspar, kaolin and zircon are crushed and ground, and then the feldspar, kaolin and zircon are put into a ball milling jar of a ball milling equipment together with the remaining solid raw materials for ball milling for 1-2 hours, and the ball milling jar is heated to make the glaze particles more tiny and uniform; then the powder is soaked in deionized water, and the mixed solution is stirred for 0.5-0.6 hours by a high-speed stirrer to form a glaze slurry; in the present invention, zirconium silicate is added to the ceramic glaze so that the strength, wear resistance, hydrolysis resistance and corrosion resistance of the ceramic glaze layer are improved, and the graphene oxide has excellent acid and alkali resistance, and can effectively improve the corrosion resistance of the ceramic glaze.

[0006] CN117049895A discloses a plain rock glaze and a preparation method thereof and a tile, wherein the plain rock glaze comprises potassium feldspar, sodium feldspar, quartz, calcined kaolin, kaolin, mica particles, calcined zinc oxide, corundum, calcined talc and zirconium silicate. The present invention optimizes the raw materials and the proportions, so that the glaze surface prepared by using the glaze is matte, and under the irradiation of soft non-reflective light, the tile surface presents fine and evenly distributed metallic luster, and the glaze surface is dotted with stars, shining like a vast galaxy, and the glaze surface after polishing looks smooth and soft, but has a fine granular touch, has excellent anti-skid, anti-slip effect, anti-fouling performance, and the glaze surface is wear-resistant, high in hardness, clear and not hazy, and has very high comprehensive performance.

[0007] In order to improve the mechanical properties and wear resistance of ceramics, they can be improved by adding additives, etc., so there is an urgent need to provide a new ceramic glaze to solve the above problems. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the defects and shortcomings in the prior art and provide a green and environmentally friendly ceramic glaze and a preparation method thereof. The glaze comprises the following components in parts by weight: 50 to 70 parts of attapulgite; 20 to 40 parts of bentonite; 10 to 30 parts of zircon; 5 to 15 parts of quartz; 4 to 10 parts of calcium feldspar; 3 to 5 parts of pyrolusite; 2 to 6 parts of molybdenum oxide; 4 to 8 parts of melamine; 1 to 3 parts of polyvinyl alcohol 2000; and 40 to 60 parts of water. The mechanical properties of the glaze layer can be improved by adding quartz and calcium feldspar, while calcium feldspar affects the stability of zircon production of ZrO2; the mechanical properties are further improved by adding pyrolusite and MoO3 composite to catalyze the production of mullite, and the added melamine can produce aluminum nitride with aluminum under high temperature conditions, thereby improving the mechanical properties and wear resistance of the glaze layer.

[0009] The purpose of the invention is to provide a green and environmentally friendly ceramic glaze.

[0010] Another object of the present invention is to provide a method for preparing a green and environmentally friendly ceramic glaze.

[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0012] A green and environmentally friendly ceramic glaze comprises the following components in parts by weight: 50-70 parts of attapulgite; 20-40 parts of bentonite; 10-30 parts of zircon; 5-15 parts of quartz; 4-10 parts of calcium feldspar; 3-5 parts of pyrolusite; 2-6 parts of molybdenum oxide; 4-8 parts of melamine; 1-3 parts of polyvinyl alcohol 2000; and 40-60 parts of water.

[0013] Preferably, the glaze comprises the following components in parts by weight: 60 parts of attapulgite; 30 parts of bentonite; 20 parts of zircon; 10 parts of quartz; 8 parts of calcium feldspar; 4 parts of pyrolusite; 4 parts of molybdenum oxide; 6 parts of melamine; 2 parts of polyvinyl alcohol 2000; and 50 parts of water.

[0014] More preferably, the particle size of the attapulgite is 40 to 80 μm; and the particle size of the bentonite is 30 to 50 μm.

[0015] More preferably, the particle size of the zircon is 20-40 μm; the particle size of the quartz is 45-65 μm.

[0016] Further preferably, the particle size of the calcium feldspar is at least one of 0.5 μm, 10 μm, and 80 μm; the particle size of the pyrolusite is 10 to 30 μm; and the particle size of the molybdenum oxide is 50 to 150 nm.

[0017] Based on the above-mentioned method for preparing a green and environmentally friendly ceramic glaze, the preparation method comprises the following steps:

[0018] 1) grinding attapulgite, bentonite, zircon, quartz, anorthite and pyrolusite respectively, sieving, and then placing the above components and water in a ball mill for ball milling and mixing;

[0019] 2) Then, melamine and polyvinyl alcohol 2000 are added into the ball milling jar and ball milling is continued to obtain a glaze.

[0020] Preferably, in step (1), the sieving is through a 200-400 mesh sieve; the ball milling time is 5-10 hours, and the ball milling speed is 200-400 r / min.

[0021] Preferably, in step (2), the ball milling time is 1 to 3 hours.

[0022] The present invention has the following beneficial effects:

[0023] The mechanical properties of the glaze layer can be improved by adding quartz and calcium feldspar, and calcium feldspar affects the stability of zircon production of ZrO2; the mechanical properties can be further improved by adding pyrolusite and MoO3 composite to catalyze the production of mullite, and the added melamine can produce aluminum nitride under high temperature conditions with aluminum, thereby improving the mechanical properties and wear resistance of the glaze layer. DETAILED DESCRIPTION

[0024] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0025] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0026] Example 1

[0027] A green and environmentally friendly ceramic glaze comprises the following components in parts by weight: 70 parts of attapulgite; 20 parts of bentonite; 30 parts of zircon; 5 parts of quartz; 10 parts of calcium feldspar; 3 parts of pyrolusite; 6 parts of molybdenum oxide; 4 parts of melamine; 3 parts of polyvinyl alcohol 2000; and 60 parts of water.

[0028] The particle size of the attapulgite is 80 μm;

[0029] The particle size of the bentonite is 30 μm;

[0030] The particle size of the zircon is 40 μm;

[0031] The particle size of the quartz is 45 μm;

[0032] The particle size of the calcium feldspar is 80 μm;

[0033] The particle size of the pyrolusite is 10 μm;

[0034] The particle size of the molybdenum oxide is 150 nm;

[0035] A method for preparing green and environmentally friendly ceramic glaze:

[0036] 1) grinding attapulgite, bentonite, zircon, quartz, anorthite and pyrolusite at a rotation speed of 400 r / min for 5 h, passing through a 300-mesh sieve, and then placing the above components and water in a ball mill for ball milling and mixing;

[0037] 2) Then, melamine and polyvinyl alcohol 2000 were added into the ball mill and ball milling was continued for 1 hour to obtain a glaze.

[0038] Example 2

[0039] A green and environmentally friendly ceramic glaze comprises the following components in parts by weight: 60 parts of attapulgite; 30 parts of bentonite; 20 parts of zircon; 10 parts of quartz; 8 parts of calcium feldspar; 4 parts of pyrolusite; 4 parts of molybdenum oxide; 6 parts of melamine; 2 parts of polyvinyl alcohol 2000; and 50 parts of water.

[0040] The particle size of the attapulgite is 60 μm;

[0041] The particle size of the bentonite is 40 μm;

[0042] The particle size of the zircon is 40 μm;

[0043] The particle size of the quartz is 55 μm;

[0044] The particle size of the calcium feldspar is 10 μm;

[0045] The particle size of the pyrolusite is 20 μm;

[0046] The particle size of the molybdenum oxide is 100 nm;

[0047] A method for preparing green and environmentally friendly ceramic glaze:

[0048] 1) grinding attapulgite, bentonite, zircon, quartz, anorthite and pyrolusite at a speed of 300 r / min for 8 h, respectively, passing through a 300-mesh sieve, and then placing the above components and water in a ball mill for ball milling and mixing; 2) then adding melamine and polyvinyl alcohol 2000 into the ball mill and continuing ball milling for 2 h to obtain a glaze.

[0049] Example 3

[0050] A green and environmentally friendly ceramic glaze comprises the following components in parts by weight: 50 parts of attapulgite; 40 parts of bentonite; 10 parts of zircon; 15 parts of quartz; 4 parts of calcium feldspar; 5 parts of pyrolusite; 2 parts of molybdenum oxide; 8 parts of melamine; 1 part of polyvinyl alcohol 2000; and 40 parts of water.

[0051] The particle size of the attapulgite is 40 μm;

[0052] The particle size of the bentonite is 50 μm;

[0053] The particle size of the zircon is 20 μm;

[0054] The particle size of the quartz is 65 μm;

[0055] The particle size of the calcium feldspar is 0.5 μm;

[0056] The particle size of the pyrolusite is 30 μm;

[0057] The particle size of the molybdenum oxide is 50 nm;

[0058] A method for preparing green and environmentally friendly ceramic glaze:

[0059] 1) grinding attapulgite, bentonite, zircon, quartz, anorthite and pyrolusite at a speed of 200 r / min for 10 h, respectively, passing through a 200-mesh sieve, and then placing the above components and water in a ball mill for ball milling and mixing;

[0060] 2) Then, melamine and polyvinyl alcohol 2000 were added into the ball mill and ball milling was continued for 3 hours to obtain a glaze.

[0061] Example 4

[0062] Example 4 is basically the same as Example 2, except that: the particle sizes of the anorthite are 10 μm and 80 μm; and the mass ratio of the 10 μm anorthite to the 80 μm anorthite is 3:1.

[0063] Example 5

[0064] Example 5 is basically the same as Example 4, except that: the particle sizes of the anorthite are 0.5 μm, 10 μm and 80 μm; the mass ratio of the 0.5 μm anorthite, 10 μm anorthite and 80 μm anorthite is 1:2:1.

[0065] Comparative Example 1

[0066] Example 1 is substantially the same as Example 2, except that 18 parts of quartz are used instead of 10 parts of quartz and 8 parts of anorthite.

[0067] Comparative Example 2

[0068] Comparative Example 2 is substantially the same as Example 2, except that 8 parts of pyrolusite are used to replace 4 parts of pyrolusite and 4 parts of molybdenum oxide.

[0069] Comparative Example 3

[0070] Comparative Example 3 is substantially the same as Example 2, except that it does not contain melamine.

[0071] The properties of the glazes of Examples 1-3 and Comparative Examples 1-4 were tested in the following manner:

[0072] 1) applying glaze to the surface of a daily-use ceramic body, and drying the body to obtain a glazed daily-use ceramic body;

[0073] 2) The glazed daily-use ceramic body is heated from room temperature to 500°C at a heating rate of 5°C / min, kept at that temperature for 3 hours, then heated to 1350°C at a heating rate of 9°C / min, and sintered for 4 hours; finally, the temperature is lowered to 800°C, kept at that temperature for 2 hours, and then cooled to room temperature to obtain the product.

[0074] The flexural strength is tested according to GB / T 4741-1999;

[0075] The tribological properties of the samples were tested using a ball-on-disc friction machine.

[0076] The specific parameter results are shown in the table below:

[0077] Flexural strength(MPa) <![CDATA[Wear rate (×10 -4 )]]> Example 1 123.5 2.7 Example 2 125.6 2.3 Example 3 121.2 2.9 Example 4 126.1 2.1 Example 5 129.3 1.6 Comparative Example 1 110.4 4.1 Comparative Example 2 113.7 3.8 Comparative Example 3 102.9 4.6

[0078] By comparing Examples 1-5 with Comparative Examples 1-3, the flexural strength and wear resistance of quartz and calcium feldspar are significantly improved compared with quartz alone; the mechanical properties are significantly improved by the combined use of pyrolusite and MoO3, while the mechanical properties and wear resistance of the glaze layer decrease after omitting melamine.

[0079] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A green and environmentally friendly ceramic glaze, characterized by: The glaze comprises the following components in parts by weight: 50-70 parts of attapulgite; 20-40 parts of bentonite; 10-30 parts of zircon; 5-15 parts of quartz; 4-10 parts of calcium feldspar; 3-5 parts of pyrolusite; 2-6 parts of molybdenum oxide; 4-8 parts of melamine; and 1-3 parts of polyvinyl alcohol 2000. 40-60 parts of water; The particle size of the attapulgite is 40 to 80 μm; the particle size of the bentonite is 30 to 50 μm; The particle size of the zircon is 20 to 40 μm; the particle size of the quartz is 45 to 65 μm; The particle sizes of the calcium feldspar are 0.5 μm, 10 μm and 80 μm; the mass ratio of the calcium feldspar of 0.5 μm, 10 μm and 80 μm is 1:2:1; the particle size of the pyrolusite is 10-30 μm; and the particle size of the molybdenum oxide is 50-150 nm.

2. The green and environmentally friendly ceramic glaze according to claim 1, characterized in that: The glaze comprises the following components in parts by weight: 60 parts of attapulgite; 30 parts of bentonite; 20 parts of zircon; Quartz 10 parts; 8 parts of calcium feldspar; 4 parts of pyrolusite; 4 parts of molybdenum oxide; 6 parts of melamine; 2 parts of polyvinyl alcohol 2000; 50 parts of water.

3. The method for preparing a green and environmentally friendly ceramic glaze according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: 1) grinding attapulgite, bentonite, zircon, quartz, anorthite and pyrolusite respectively, sieving, and then placing the above components and water in a ball mill for ball milling and mixing; 2) Then, melamine and polyvinyl alcohol 2000 are added into the ball milling jar and ball milling is continued to obtain a glaze.

4. The method for preparing a green and environmentally friendly ceramic glaze according to claim 3, characterized in that: In step 1), the sieving is through a 200-400 mesh sieve; the ball milling time is 5-10 hours, and the ball milling speed is 200-400 r / min.

5. The method for preparing a green and environmentally friendly ceramic glaze according to claim 3, characterized in that: In step 2), the ball milling time is 1 to 3 hours.