RGO modified polymer emulsion and preparation method thereof, mortar composition, electromagnetic shielding waterproof mortar and preparation method thereof
Through the synergistic effect of graphene oxide modified polymer emulsion and cement and other components, the mechanical properties and electromagnetic shielding efficiency of electromagnetic shielding waterproof mortar are improved, solving the problem of insufficient performance of electromagnetic shielding cement mortar in the existing technology, and achieving high efficiency , Environmentally friendly electromagnetic shielding effect.
Patent Information
- Application Number
- CN202311772887.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-12-21
AI Technical Summary
Existing electromagnetic shielding cement mortars cannot combine high mechanical properties and excellent electromagnetic shielding efficiency, and traditional metal materials have problems such as environmental pollution and weight increase.
RGO modified polymer emulsion is prepared through reduction treatment using graphene oxide modified polymer emulsion, and mixed with Portland cement and other components to form electromagnetic shielding waterproof mortar to improve its electromagnetic shielding efficiency, flexural strength, and compression resistance. Strength and bonding strength.
The prepared electromagnetic shielding waterproof mortar has the highest shielding efficiency of not less than 31dB, flexural strength of not less than 8.0MPa, compressive strength of not less than 28.6MPa, bonding strength of not less than 1.55MPa, no metal powder, and environmentally friendly ingredients , suitable for places with dense electronic equipment.
Smart Images

Figure BDA0004621722070000091 
Figure BDA0004621722070000141 
Figure BDA0004621722070000151
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to an RGO modified polymer emulsion and a preparation method thereof, a mortar composition, an electromagnetic shielding waterproof mortar and a preparation method thereof. Background Art
[0002] At present, the electromagnetic shielding materials in electromagnetic shielding cement mortar are generally carbon black, graphite, metal powder, conductive fiber, etc. This type of material has good conductivity, but poor shielding ability for low-frequency magnetic fields, and the components of electromagnetic shielding cement mortar are relatively single, and the overall electromagnetic shielding performance is poor. Moreover, some metal powders (such as lead) are polluting to the environment. Adding traditional metal materials to cement-based materials may increase the weight of the mortar and cause metal corrosion problems.
[0003] CN115259781A discloses an electromagnetic shielding mortar which is composed of cementitious materials, water, river sand, nano-iron tetroxide, micron-iron tetroxide and polycarboxylic acid high-efficiency water reducing agent. The proportion of each material is: cementitious material 831.79kg / m 3 、Water 340.47kg / m 3 、River sand 987.24kg / m 3 、Nano ferroferric oxide 19.90kg / m 3 、Micron FeO4 49.75kg / m 3 And polycarboxylate high efficiency water reducing agent 0.90kg / m 3 This invention effectively improves the electromagnetic shielding performance of cement mortar by adding nano- and micron-sized ferroferric oxide. However, the price of nano-ferroferric oxide is extremely high, and it has the disadvantages of easy agglomeration. Improper construction and storage will have a great impact on the electromagnetic shielding effect of the final mortar.
[0004] CN116217148A discloses an electromagnetic shielding cement mortar and its preparation method. The electromagnetic shielding cement mortar is composed of the following raw materials by mass: 15-50 parts of cement, 0.05-0.2 parts of water-retaining thickener, 0-2 parts of additives, 0.03-0.2 parts of accelerator, 50-80 parts of electromagnetic shielding filler and 10-30 parts of water. The electromagnetic shielding filler includes graphite, carbon black, carbon fiber, iron oxide and iron-based microcrystalline alloy powder; wherein the content of the iron oxide is greater than 70%, and the content of the iron-based microcrystalline alloy powder is greater than 5%. This invention has good high electromagnetic shielding efficiency, and at the same time broadens the electromagnetic shielding band, and has a better protective effect on low-frequency electromagnetic radiation. However, the content of the electromagnetic shielding material used is extremely high, and the compressive strength and bonding strength of this type of cement mortar are not high, which easily leads to hollowing, cracking and falling off. At the same time, the iron-based microcrystalline alloy powder may be oxidized, rusted, etc., resulting in a decrease in the mechanical properties and electromagnetic shielding effect of the mortar. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem that the electromagnetic shielding waterproof mortar in the prior art cannot have both high mechanical properties and excellent electromagnetic shielding effectiveness.
[0006] In order to achieve the above object, the present invention provides a method for preparing a GO-modified polymer emulsion, characterized in that it comprises the following steps:
[0007] S1: performing a first mixing treatment on a graphene oxide dispersion and a polymer emulsion to obtain a graphene oxide modified polymer emulsion;
[0008] S2: performing a second mixing treatment on the graphene oxide modified polymer emulsion and a reducing agent to obtain an RGO modified polymer emulsion;
[0009] Wherein, in step S1, the polymer emulsion is styrene-acrylic emulsion and / or styrene-butadiene emulsion;
[0010] In step S2, the reducing agent is selected from at least one of ascorbic acid, glucose, hydrazine hydrate and sodium borohydride.
[0011] The second aspect of the present invention provides an RGO modified polymer emulsion prepared by the preparation method provided by the first aspect of the present invention.
[0012] The third aspect of the present invention provides a mortar composition, comprising component A and component B, wherein component A comprises RGO modified polymer emulsion, defoamer, and bactericide, and component B comprises silicate cement, active filler, barite, quartz sand, barium sulfate, cellulose ether, water reducer, water repellent, carbon fiber, and silicon carbide fiber;
[0013] Wherein, the RGO modified polymer emulsion is the RGO modified polymer emulsion provided in the second aspect of the present invention.
[0014] The fourth aspect of the present invention provides a method for preparing an electromagnetic shielding waterproof mortar, which is carried out using the mortar composition provided by the third aspect of the present invention, and comprises the following steps:
[0015] S1: performing a third mixing process on the components in component A to obtain a mixture A; and performing a fourth mixing process on the components in component B to obtain a mixture B;
[0016] S2: Perform a fifth mixing process on mixture A and mixture B to obtain an electromagnetic shielding waterproof mortar.
[0017] The fifth aspect of the present invention provides an electromagnetic shielding waterproof mortar prepared by the preparation method provided by the fourth aspect of the present invention.
[0018] The preparation method of the RGO modified polymer emulsion provided by the present invention has simple preparation steps and easily controllable parameters. The prepared RGO modified polymer emulsion is used in electromagnetic shielding waterproof mortar, which can simultaneously improve the electromagnetic shielding effectiveness, flexural strength, compressive strength and bonding strength of the electromagnetic shielding waterproof mortar.
[0019] The mortar composition provided by the present invention has synergistic effects among its components, and the obtained electromagnetic shielding waterproof mortar has a maximum shielding effectiveness of not less than 31dB, a flexural strength of not less than 8.0MPa, a compressive strength of not less than 28.6MPa, and a bonding strength of not less than 1.55MPa. In addition, the mortar composition provided by the present invention contains no metal powder and has environmentally friendly ingredients, so the obtained electromagnetic shielding waterproof mortar is environmentally friendly. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] It should be noted that, in the present invention, the RGO represents reduced graphene oxide, and the GO represents graphene oxide;
[0022] It should also be noted that, in the present invention, normal temperature refers to 25°C±5°C, and normal pressure refers to 101KPa.
[0023] As mentioned above, the first aspect of the present invention provides a method for preparing a RGO modified polymer emulsion, characterized in that it comprises the following steps:
[0024] S1: performing a first mixing treatment on a graphene oxide dispersion and a polymer emulsion to obtain a graphene oxide modified polymer emulsion;
[0025] S2: performing a second mixing treatment on the graphene oxide modified polymer emulsion and a reducing agent to obtain an RGO modified polymer emulsion;
[0026] Wherein, in step S1, the polymer emulsion is styrene-acrylic emulsion and / or styrene-butadiene emulsion;
[0027] In step S2, the reducing agent is selected from at least one of ascorbic acid, glucose, hydrazine hydrate and sodium borohydride.
[0028] The inventors of the present invention have found that after the graphene oxide dispersion is mixed and modified with the polymer emulsion, the graphene oxide modified polymer emulsion is then reduced by a reducing agent, and the obtained RGO modified polymer emulsion has good interlocking force with the cement hydration product, which can increase the density of the hydration product, optimize the microstructure of the hydration product, and improve the mechanical properties of the mortar. In addition, the RGO in the RGO modified polymer emulsion obtained by the preparation method provided by the present invention will overlap with each other to form a good interface, thereby significantly improving the electromagnetic shielding effectiveness of the mortar.
[0029] Particularly preferably, the reducing agent is ascorbic acid.
[0030] It should be noted that the present invention has no special requirements on the preparation method of the graphene oxide dispersion, and the graphene oxide dispersion can be prepared by the preparation method conventionally used by those skilled in the art.
[0031] Exemplarily, the graphene oxide dispersion can be prepared according to but not limited to the following steps:
[0032] S01: mixing graphite and sodium nitrate at a mixing temperature not higher than 5° C. to obtain a mixed solution I;
[0033] S02: under the condition that the mixing temperature is not higher than 5°C, add concentrated sulfuric acid to the mixed solution I, react for 30min-60min, and obtain a mixed solution II;
[0034] S03: adding potassium permanganate to the mixed solution II, reacting at a reaction temperature of 30°C-40°C for 20min-40min to obtain a mixed solution III;
[0035] S04: adding water to the mixed solution III, reacting at a reaction temperature of 90°C-100°C for 20min-30min to obtain a mixed solution IV;
[0036] S05: adding hydrogen peroxide to the mixed solution IV, allowing it to stand, separating the precipitate and washing it to obtain graphene oxide;
[0037] S06: preparing the graphene oxide into a graphene oxide dispersion having a desired concentration.
[0038] According to some preferred embodiments of the present invention, the content of graphene oxide in the graphene oxide dispersion is 10g / L-50g / L, the amount of the polymer emulsion is 200g-400g, and the amount of the reducing agent is 10g-100g per 1L of the graphene oxide dispersion. Under this preferred condition, the prepared RGO modified polymer emulsion can further improve the electromagnetic shielding effectiveness and mechanical properties of the electromagnetic shielding waterproof mortar.
[0039] According to some particularly preferred embodiments of the present invention, in step S1, the polymer emulsion is a styrene-acrylic emulsion and a styrene-butadiene emulsion in a mass ratio of 0.5-2:1. Under this preferred condition, the prepared RGO modified polymer emulsion can further improve the electromagnetic shielding effectiveness and mechanical properties of the electromagnetic shielding waterproof mortar.
[0040] According to a particularly preferred embodiment of the present invention, in step S1, the graphene oxide dispersion further comprises a dispersant, and the dispersant is selected from at least one of polyacrylates, polyphosphates, and polycarboxylates.
[0041] Further preferably, in the graphene oxide dispersion, the content of the dispersant is 1 g / L-3 g / L.
[0042] According to some preferred embodiments of the present invention, in step S1, the solid content of the styrene-acrylic emulsion is 47 wt%-49 wt%, and the viscosity at 25°C is 10 mPa·s-90 mPa·s.
[0043] According to some preferred embodiments of the present invention, in step S1, the solid content of the styrene-butadiene emulsion is 49 wt%-51 wt%, and the viscosity is 10 mPa·s-90 mPa·s at 25°C.
[0044] According to a particularly preferred embodiment of the present invention, in step S2, the reducing agent is ascorbic acid.
[0045] It should be noted that the present invention has no particular limitation on the conditions of the first mixing treatment and the second mixing treatment. For example, sufficient mixing can be performed under normal temperature and pressure.
[0046] The second aspect of the present invention provides an RGO modified polymer emulsion prepared by the preparation method provided by the first aspect of the present invention.
[0047] The third aspect of the present invention provides a mortar composition, comprising component A and component B, wherein component A comprises RGO modified polymer emulsion, defoamer, and bactericide, and component B comprises silicate cement, active filler, barite, quartz sand, barium sulfate, cellulose ether, water reducer, water repellent, carbon fiber, and silicon carbide fiber;
[0048] Wherein, the RGO modified polymer emulsion is the RGO modified polymer emulsion provided in the second aspect of the present invention.
[0049] The inventors of the present invention have discovered that the RGO modified polymer emulsion provided in the second aspect of the present invention can produce a synergistic effect with other components in the mortar composition, thereby improving the mechanical properties and electromagnetic shielding effectiveness of the prepared electromagnetic shielding waterproof mortar.
[0050] The RGO modified polymer emulsion provided in the second aspect of the present invention can form an effective conductive network structure with carbon fibers and silicon carbon fibers, thereby enhancing the internal magnetic field of the mortar and further improving the electromagnetic shielding effectiveness of the mortar.
[0051] According to some preferred embodiments of the present invention, the mass ratio of the component A to the component B is 1:3-4.
[0052] According to some preferred embodiments of the present invention, the component A further comprises water. Based on the total mass of the component A as 100 parts by mass, the content of the RGO modified polymer emulsion is 80-90 parts by mass, the content of the defoamer is 0.1-0.5 parts by mass, the content of the bactericide is 0.2-0.4 parts by mass, and the content of water is 7-20 parts by mass.
[0053] According to some preferred embodiments of the present invention, based on the total mass of the B component as 100 parts by mass, the content of the silicate cement is 30-50 parts by mass, the content of the active filler is 2-5 parts by mass, the content of the barite is 10-20 parts by mass, the content of the quartz sand is 20-30 parts by mass, the content of the barium sulfate is 10-20 parts by mass, the content of the cellulose ether is 0.1-0.3 parts by mass, the content of the water reducer is 0.1-0.2 parts by mass, the content of the water repellent is 0.1-0.2 parts by mass, the content of the carbon fiber is 0.2-0.4 parts by mass, and the content of the silicon carbide fiber is 0.2-0.4 parts by mass.
[0054] Particularly preferably, the average single fiber diameter of the carbon fiber is 3 μm-5 μm, and the average single fiber length is 4 mm-8 mm.
[0055] Particularly preferably, the average single fiber diameter of the silicon carbide fiber is 0.1 μm-2.5 μm, and the average single fiber length is 10 μm-50 μm.
[0056] According to some preferred embodiments of the present invention, the defoaming agent is an organosilicon defoaming agent.
[0057] According to some preferred embodiments of the present invention, the fungicide is selected from at least one of 1,2-benzisothiazolinone, methylisothiazolinone and methylchloroisothiazolinone.
[0058] According to some preferred embodiments of the present invention, the silicate cement is selected from at least one of PII42.5 silicate cement, P.O42.5R ordinary silicate cement, P.W32.5 white silicate cement, P.W52.5 white silicate cement, and PC32.5 composite silicate cement.
[0059] According to some preferred embodiments of the present invention, the active filler is selected from at least one of metakaolin, silica fume and fly ash.
[0060] According to some preferred embodiments of the present invention, the average particle diameter of the barite is 40 mesh to 120 mesh.
[0061] According to some preferred embodiments of the present invention, the average particle diameter of the quartz sand is 70 mesh to 120 mesh.
[0062] According to some preferred embodiments of the present invention, the average particle diameter of the barium sulfate is 800 mesh to 1250 mesh.
[0063] According to some preferred embodiments of the present invention, the cellulose ether is hydroxyethyl methylcellulose and / or hydroxypropyl methylcellulose.
[0064] According to some preferred embodiments of the present invention, the water reducer is selected from at least one of polycarboxylate water reducer, melamine water reducer and lignin sulfonate.
[0065] According to some preferred embodiments of the present invention, the water repellent is a silicone water repellent.
[0066] The fourth aspect of the present invention provides a method for preparing an electromagnetic shielding waterproof mortar, which is carried out using the mortar composition provided by the third aspect of the present invention, and comprises the following steps:
[0067] S1: performing a third mixing process on the components in component A to obtain a mixture A; and performing a fourth mixing process on the components in component B to obtain a mixture B;
[0068] S2: Perform a fifth mixing process on mixture A and mixture B to obtain an electromagnetic shielding waterproof mortar.
[0069] According to some preferred embodiments of the present invention, the third mixing treatment at least meets the following requirements: temperature of 5°C-35°C, stirring rate of 300r / min-1000r / min, and time of 10min-30min.
[0070] According to some preferred embodiments of the present invention, the fourth mixing treatment at least meets the following requirements: temperature of 5°C-35°C, stirring rate of 300r / min-500r / min, and time of 10min-30min.
[0071] According to some preferred embodiments of the present invention, the fifth mixing treatment at least meets the following requirements: temperature of 5°C-35°C, stirring rate of 500r / min-1000r / min, and time of 2min-3min.
[0072] The fifth aspect of the present invention provides an electromagnetic shielding waterproof mortar prepared by the preparation method provided by the fourth aspect of the present invention.
[0073] The electromagnetic shielding waterproof mortar provided by the present invention is suitable for places with electromagnetic wave interference and requiring waterproofing, such as hospitals, laboratories, computer rooms, TV towers and other places with dense electronic equipment. It can also be used in home decoration. It can not only be waterproof, but also reduce the impact of electromagnetic radiation on the human body.
[0074] The present invention will be described in detail below through examples. In the following examples, the instruments, reagents, materials, etc. involved, unless otherwise specified, are all conventional instruments, reagents, materials, etc. already in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following examples, unless otherwise specified, are all conventional experimental methods, detection methods, etc. already in the prior art.
[0075] In the following examples, normal temperature means 25°C ± 5°C, and normal pressure means 101KPa.
[0076] In the following examples, the property parameters and sources of each raw material are shown in Table 1:
[0077] Table 1
[0078]
[0079] Preparation Example 1
[0080] S0: Preparation of graphene oxide dispersion with a graphene oxide content of 30 mg / mL
[0081] S01: 2 g of graphite and 2 g of sodium nitrate were mixed at a mixing temperature of 5°C to obtain a mixed solution I;
[0082] S02: Under the condition of a mixing temperature of 5°C, 100 ml of concentrated sulfuric acid (concentration of 98 wt%) was added to the mixed solution I, and the mixture was stirred for reaction for 40 min to obtain a mixed solution II;
[0083] S03: Add 6 g of potassium permanganate to the mixed solution II, and react at a reaction temperature of 35° C. for 30 min to obtain a mixed solution III;
[0084] S04: Add 200 ml of distilled water to the mixed solution III, and react at a reaction temperature of 97° C. for 15 min to obtain a mixed solution IV;
[0085] S05: After adding 20 ml of hydrogen peroxide to the mixed solution IV, the mixture was allowed to stand, the precipitate was separated and the precipitate was washed to obtain graphene oxide;
[0086] S06: mixing the graphene oxide, the dispersant and water to prepare a graphene oxide dispersion having a graphene oxide concentration of 30 mg / mL, wherein the content of the dispersant in the graphene oxide dispersion is 2 g / L.
[0087] S1: performing a first mixing treatment on the graphene oxide dispersion and the polymer emulsion to obtain a graphene oxide modified polymer emulsion.
[0088] S2: performing a second mixing treatment on the graphene oxide modified polymer emulsion and a reducing agent to obtain an RGO modified polymer emulsion A1.
[0089] Specifically, with respect to every 1L of graphene oxide dispersion, the amount of the polymer emulsion is 300g, the amount of the reducing agent is 50g, the polymer emulsion is a styrene acrylic emulsion, and the reducing agent is ascorbic acid;
[0090] The first mixing process and the second mixing process are performed under normal temperature and pressure conditions.
[0091] Preparation Example 2
[0092] The method of Example 1 was followed, except that the polymer emulsion was styrene-butadiene emulsion, to obtain RGO-modified polymer emulsion A2.
[0093] Preparation Example 3
[0094] The method of Example 1 was followed, except that the polymer emulsion was a styrene-acrylic emulsion and a styrene-butadiene emulsion in a mass ratio of 1:1, to obtain an RGO-modified polymer emulsion A3.
[0095] Preparation Example 4
[0096] The method of Example 1 was followed, except that, relative to 1 L of graphene oxide dispersion, the amount of the polymer emulsion was 500 g, and the amount of the reducing agent was 8 g, to obtain RGO modified polymer emulsion A4.
[0097] Comparative Preparation Example 1
[0098] The method of Example 1 is followed, except that step S2 is not performed. Specifically, the preparation steps are as follows:
[0099] S0: Prepare a graphene oxide dispersion with a graphene oxide content of 30 mg / mL, with the specific steps and parameters being the same as those in Example 1.
[0100] S1: The graphene oxide dispersion and the polymer emulsion are subjected to a first mixing treatment to obtain a graphene oxide modified polymer emulsion DA1. Specifically, the amount of the polymer emulsion used is 300 g per 1 L of the graphene oxide dispersion, and the polymer emulsion is a styrene acrylic emulsion. The first mixing treatment and the second mixing treatment are carried out at normal temperature and pressure.
[0101] Comparative Preparation Example 2
[0102] The method of Example 1 is followed, except that the graphene oxide dispersion is first subjected to reduction treatment and then mixed with the polymer emulsion. Specifically, the preparation steps are as follows:
[0103] S0: Prepare a graphene oxide dispersion with a graphene oxide content of 30 mg / mL, with the specific steps and parameters being the same as those in Example 1.
[0104] S1: performing a first mixing treatment on the graphene oxide dispersion and the reducing agent to obtain a reduced graphene oxide dispersion.
[0105] S2: performing a second mixing treatment on the reduced graphene oxide dispersion and the polymer emulsion to obtain an RGO-modified polymer emulsion DA2.
[0106] Specifically, with respect to every 1L of graphene oxide dispersion, the amount of the polymer emulsion is 300g, the amount of the reducing agent is 50g, the polymer emulsion is a styrene acrylic emulsion, and the reducing agent is ascorbic acid;
[0107] The first mixing process and the second mixing process are performed under normal temperature and pressure conditions.
[0108] Example 1
[0109] S1: performing a third mixing process on the components in component A of the mortar composition to obtain a mixture A; and performing a fourth mixing process on the components in component B of the mortar composition to obtain a mixture B;
[0110] S2: Mixture A and mixture B are subjected to a fifth mixing process to obtain an electromagnetic shielding waterproof mortar B1.
[0111] Specifically, the stirring rate of the third mixing process is 900 rpm, the stirring time is 20 min, and the temperature is 25°C; the stirring rate of the fourth mixing process is 300 rpm, the stirring time is 15 min, and the temperature is 25°C; the stirring rate of the fifth mixing process is 850 rpm, the stirring time is 2 min, and the temperature is 25°C;
[0112] The composition ratio of the mortar composition is shown in Table 2 below.
[0113] Example 2
[0114] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by the RGO modified polymer emulsion A2, and the mass ratio of each component in the mortar composition is adjusted. Specifically, the component ratio of the mortar composition used in this example is shown in Table 2 below.
[0115] Example 3
[0116] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by the RGO modified polymer emulsion A3. Specifically, the component ratios of the mortar composition used in each example are shown in Table 2 below.
[0117] Example 4
[0118] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by the RGO modified polymer emulsion A4. Specifically, the component ratios of the mortar composition used in each example are shown in Table 2 below.
[0119] Comparative Example 1
[0120] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by the graphene oxide modified polymer emulsion DA1. Specifically, the component ratios of the mortar composition used in each comparative example are shown in Table 2 below.
[0121] Comparative Example 2
[0122] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by the RGO modified polymer emulsion DA2. Specifically, the component ratios of the mortar composition used in each comparative example are shown in Table 2 below.
[0123] Comparative Example 3
[0124] The method of Example 1 is followed, except that the carbon fibers in the mortar composition are replaced with an equal amount of carbon silicon fibers.
[0125] Specifically, the composition ratio of the mortar composition used in this comparative example is shown in Table 2 below.
[0126] Comparative Example 4
[0127] The method of Example 1 is followed, except that the carbon silicon fiber in the mortar composition is replaced by an equal amount of carbon fiber.
[0128] Specifically, the composition ratio of the mortar composition used in this comparative example is shown in Table 2 below.
[0129] Comparative Example 5
[0130] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced by a styrene acrylic emulsion.
[0131] Comparative Example 6
[0132] The method of Example 1 is followed, except that the RGO modified polymer emulsion A1 in the mortar composition is replaced with a styrene acrylic emulsion, and silicon fiber and carbon silicon fiber are not added.
[0133] Table 2
[0134] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Component A Polymer Emulsion A1 A2 A3 A4 DA1 Mass 90 80 Same as Example 1 Same as Example 1 Same as Example 1 Defoaming agent / mass 0.3 0.1 Same as Example 1 Same as Example 1 Same as Example 1 Bactericide / mass 0.2 0.2 Same as Example 1 Same as Example 1 Same as Example 1 Water / mass 9.5 19.7 Same as Example 1 Same as Example 1 Same as Example 1 Component B Portland cement / mass 45.5 40 Same as Example 1 Same as Example 1 Same as Example 1 Active filler / mass 3.5 5 Same as Example 1 Same as Example 1 Same as Example 1 Barite / mass 20 10 Same as Example 1 Same as Example 1 Same as Example 1 Quartz sand / mass 20 24 Same as Example 1 Same as Example 1 Same as Example 1 Barium sulfate / mass 10 20 Same as Example 1 Same as Example 1 Same as Example 1 Cellulose ether / mass 0.2 0.2 Same as Example 1 Same as Example 1 Same as Example 1 Water reducing agent / mass 0.2 0.2 Same as Example 1 Same as Example 1 Same as Example 1 Water repellent / mass 0.1 0.1 Same as Example 1 Same as Example 1 Same as Example 1 Carbon fiber / mass 0.3 0.2 Same as Example 1 Same as Example 1 Same as Example 1 Silicon carbide fiber / mass 0.2 0.3 Same as Example 1 Same as Example 1 Same as Example 1 Component A: Component B (mass ratio) 1:3.5 Same as Example 1 Same as Example 1 Same as Example 1 Same as Example 1 Electromagnetic shielding waterproof mortar number B1 B2 B3 B4 DB1
[0135] Table 2 (Continued)
[0136]
[0137]
[0138] Test Case
[0139] The electromagnetic shielding waterproof mortars prepared in the above embodiments and comparative examples were subjected to the following mechanical property and electromagnetic shielding performance tests according to JC / T 984-2011 "Polymer cement waterproof mortar" and SJ20524-1995 "Method for measuring shielding effectiveness of materials". The results are shown in Table 3 below.
[0140] Table 3
[0141] Electromagnetic shielding waterproof mortar Flexural strength / MPa Compressive strength / MPa Adhesive strength / MPa Maximum electromagnetic shielding effectiveness / dB B1 9.5 35.7 1.74 40 B2 8.9 33.6 1.67 35 B3 10.8 39.6 1.88 43 B4 8.2 28.6 1.55 31 DB1 5.8 20.7 1.02 21 DB2 6.7 24.3 1.21 26 DB3 7.5 25.4 1.34 25 DB4 7.2 22.7 1.28 24 DB5 6.3 20.5 1.17 16 DB6 5.5 18.9 0.93 8
[0142] It can be seen from the results in Table 3 that the RGO modified polymer emulsion prepared by the preparation method provided by the present invention synergizes with other components in the waterproof mortar to obtain an electromagnetic shielding waterproof mortar with excellent mechanical properties and electromagnetic shielding effectiveness, with a flexural strength of not less than 8.0 MPa, a compressive strength of not less than 28.6 MPa, a bonding strength of not less than 1.55 MPa, and a maximum electromagnetic shielding effectiveness of not less than 31 dB. In addition, the mortar composition provided by the present invention is free of metal powder and has environmentally friendly ingredients. The obtained electromagnetic shielding waterproof mortar is environmentally friendly and is suitable for places with dense electronic equipment such as hospitals, laboratories, computer rooms, and TV towers, and has broad application prospects.
[0143] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A mortar composition, characterized in that: The invention comprises component A and component B, wherein the component A comprises RGO modified polymer emulsion, defoamer and bactericide, and the component B comprises silicate cement, active filler, barite, quartz sand, barium sulfate, cellulose ether, water reducing agent, water repellent, carbon fiber and silicon carbide fiber; Wherein, the RGO modified polymer emulsion is prepared by a preparation method comprising the following steps: S1: performing a first mixing treatment on a graphene oxide dispersion and a polymer emulsion to obtain a graphene oxide modified polymer emulsion; S2: performing a second mixing treatment on the graphene oxide modified polymer emulsion and a reducing agent to obtain an RGO modified polymer emulsion; In step S1, the polymer emulsion is a styrene-acrylic emulsion and / or a styrene-butadiene emulsion; In step S2, the reducing agent is selected from at least one of ascorbic acid, glucose, hydrazine hydrate, and sodium borohydride; The content of graphene oxide in the graphene oxide dispersion is 10 g / L-30 g / L. Relative to 1 L of graphene oxide dispersion, the amount of the polymer emulsion is 200 g-400 g, and the amount of the reducing agent is 50 g-100 g.
2. The mortar composition according to claim 1, characterized in that The mass ratio of the A component to the B component is 1:3-4.
3. The mortar composition according to claim 1 or 2, characterized in that: The component A further comprises water. Based on the total mass of the component A being 100 parts by mass, the content of the RGO modified polymer emulsion is 80-90 parts by mass, the content of the defoamer is 0.1-0.5 parts by mass, the content of the bactericide is 0.2-0.4 parts by mass, and the content of the water is 7-20 parts by mass. And / or, based on the total mass of the B component as 100 parts by mass, the content of the silicate cement is 30-50 parts by mass, the content of the active filler is 2-5 parts by mass, the content of the barite is 10-20 parts by mass, the content of the quartz sand is 20-30 parts by mass, the content of the barium sulfate is 10-20 parts by mass, the content of the cellulose ether is 0.1-0.3 parts by mass, the content of the water reducer is 0.1-0.2 parts by mass, the content of the water repellent is 0.1-0.2 parts by mass, the content of the carbon fiber is 0.2-0.4 parts by mass, and the content of the silicon carbide fiber is 0.2-0.4 parts by mass.
4. The mortar composition according to claim 1 or 2, characterized in that: The average single fiber diameter of the carbon fiber is 3 μm-5 μm, and the average single fiber length is 4 mm-8 mm; And / or, the average single fiber diameter of the silicon carbide fiber is 0.1 μm-2.5 μm, and the average single fiber length is 10 μm-50 μm.
5. The mortar composition according to claim 1 or 2, characterized in that: In step S1, the polymer emulsion is a styrene-acrylic emulsion and a styrene-butadiene emulsion in a mass ratio of 0.5-2:
1.
6. The mortar composition according to claim 1 or 2, characterized in that: In step S1, the graphene oxide dispersion further comprises a dispersant, and the dispersant is selected from at least one of polyacrylates, polyphosphates, and polycarboxylates.
7. The mortar composition according to claim 6, characterized in that: In step S1, in the graphene oxide dispersion, the content of the dispersant is 1 g / L-3 g / L.
8. The mortar composition according to claim 1 or 2, characterized in that: The solid content of the styrene-acrylic emulsion is 47wt%-49wt%, and the viscosity is 10mPa·s-90mPa·s at 25°C; And / or, the solid content of the styrene-butadiene emulsion is 49wt%-51wt%, and the viscosity at 25°C is 10mPa·s-90mPa·s.
9. A method for preparing electromagnetic shielding waterproof mortar, characterized in that: The method is carried out using the mortar composition according to any one of claims 1 to 8, comprising the following steps: S1: performing a third mixing process on the components in component A to obtain a mixture A; and performing a fourth mixing process on the components in component B to obtain a mixture B; S2: Perform a fifth mixing process on mixture A and mixture B to obtain an electromagnetic shielding waterproof mortar.
10. Electromagnetic shielding waterproof mortar prepared by the preparation method according to claim 9.