Novel ultra-soft electromagnetic shielding material, preparation method and application thereof

By coating the surface of hollow glass microspheres with conductive polymer nanomaterials and adding ZrO2-doped TiO2 composite nanoparticles, micro-conductive channels are constructed, solving the problems of lightweight and high efficiency of electromagnetic shielding materials. This results in a low-density, high-performance electromagnetic shielding material suitable for electronic devices.

CN118931187AInactive Publication Date: 2024-11-12HOHAI UNIV

Patent Information

Application Number
CN202411169282.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing electromagnetic shielding materials, while maintaining high electromagnetic shielding performance, are difficult to make lightweight and miniaturized, and traditional materials have a high density, which affects their application in electronic devices.

Method used

Hollow glass microspheres are used as the matrix, and conductive polymer nanomaterials are coated on their surface by chemical oxidation polymerization. ZrO2-doped TiO2 composite nanoparticles are added to form conductive channels. Combined with carbon aerogel and conductive polymer nanomaterials, micro-conductive channels are constructed to enhance electromagnetic shielding performance and reduce material density.

Benefits of technology

It achieves electromagnetic shielding effectiveness of 30-60dB, density of 0.4-0.8g/cm3, and has good flexibility and environmental purification capabilities, making it suitable for industrial and commercial electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931187A_ABST
    Figure CN118931187A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electromagnetic shielding materials, and discloses a novel ultra-soft electromagnetic shielding material, a preparation method and application thereof, the electromagnetic shielding material is formed by uniformly mixing a matrix and a filler; the matrix is composed of the following raw materials in parts by weight: 10-20 parts of silicone rubber; 30-60 parts of a xylene solvent; 30 to 50 parts of cobalt sulfate; 0.5 to 1.0 part of a curing agent; the filler is prepared from the following raw materials in parts by weight: 10 to 20 parts of hollow glass beads; 5-10 parts of a conductive polymer nano material; 1 to 5 parts of composite nano particles of ZrO2 doped with TiO2; 2-3 parts of an oxidant; and 3-5 parts of carbon aerogel. Dielectric parameter regulation and control reinforcement and shielding performance reinforcement can be achieved, the density of the composite material can be effectively reduced while high electromagnetic shielding effectiveness is guaranteed, the composite material has good flexibility, and in addition, the problem of abnormal damage of the hollow glass beads and the silicone rubber in the mixing process can be effectively solved through the xylene solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electromagnetic shielding materials, and in particular to a novel ultra-light and flexible electromagnetic shielding material, a preparation method and application thereof. Background Art

[0002] The rapid development of electronic information technology has brought about an efficient and convenient life. At the same time, it has also caused a lot of electromagnetic pollution, affecting the operation of precision instruments and equipment, the health of animals and plants, the security of confidential information, especially the rapidly developing 5G communication technology. In view of the above problems, the use of electromagnetic shielding materials for protection is the most economical, effective and convenient means.

[0003] Electromagnetic shielding materials, as a functional protective material that effectively isolates incident electromagnetic waves by means of reflection loss outside the material and absorption loss inside the material, have been widely used in the field of electromagnetic protection. At the same time, with the increasing miniaturization and high degree of integration of electronic components, electromagnetic leakage and interference problems in electrical equipment have become increasingly prominent. Therefore, people have put forward higher performance requirements for electromagnetic shielding materials, requiring them to be thin, light, wide and strong.

[0004] As the research on electromagnetic shielding materials has been paid more and more attention, various electromagnetic shielding materials have been developed, the main types are: metal materials, carbon materials, conductive coatings and filled composite materials. Among them, traditional metal shell materials have a high shielding efficiency for electromagnetic waves and can reflect electromagnetic waves well to achieve interference shielding. However, due to its high density, easy corrosion and secondary pollution caused by a large number of reflections, its application is limited. Relevant literature shows that silicone rubber-based filled polymer-based composite materials have received widespread attention in the field of electromagnetic shielding due to their advantages such as good corrosion resistance, easy processing and adjustable conductivity. Silicone rubber has excellent thermal stability, electrical properties and flexibility. As the base material of electromagnetic shielding composite materials, it can be used as electromagnetic shielding gasket materials in electronic equipment.

[0005] Metal fillers have excellent electrical conductivity and magnetic properties. Many studies have added them to silicone rubber matrix as electromagnetic shielding fillers. Related literature adds nickel-plated copper and silver-plated nickel to silicone rubber matrix to obtain composite materials with excellent electromagnetic shielding performance. The above two materials have good effects on electromagnetic wave shielding, but the prepared electromagnetic shielding specific gravity is relatively large, 2.5g / cm 3 and 4.2g / cm 3 , affecting its application in electronic equipment.

[0006] In addition to conductive metal fillers, carbon materials also have excellent conductive properties. Compared with metal fillers, carbon materials have lower density. Metal fillers are usually mixed and added to the silicone rubber matrix to prepare electromagnetic shielding composite materials. For example, application number CN201810686542.7 discloses a graphene-modified electromagnetic shielding silicone rubber material and its preparation method, which mixes and reacts graphene with octamethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane under an anionic catalyst to obtain graphene-silicone rubber, and then mixes with other metal conductive material components in proportion. The obtained composite material has a good effect on shielding electromagnetic waves, and the shielding effectiveness reaches 80dB at 300-1000MHz, but the material specific gravity is still relatively high, with a density of 1.80g / cm 3 .

[0007] For example, application number CN202111491590.9 discloses a method for preparing a foamed silicone rubber composite material for electromagnetic shielding, which utilizes carbon-based materials (graphene, highly conductive carbon black, etc.) to modify silicone rubber and adopts a chemical foaming method to prepare an electromagnetic shielding composite material. The material has the characteristics of simple preparation process, light weight, uniform pores, and small average pore size, but the electromagnetic shielding effectiveness is only 26.2dB.

[0008] For many occasions in aerospace and civil applications, the lightweight and miniaturization of electromagnetic shielding materials is an urgent problem to be solved while maintaining a certain electromagnetic shielding performance. Lightweight electromagnetic shielding composite materials with high electromagnetic shielding efficiency and simple preparation process (especially with a density of 1g / cm 3 The following) and its preparation process need to be explored and developed urgently.

[0009] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention

[0010] Purpose of the invention: In order to solve the problems of existing materials and preparation technologies, the present invention provides a new type of ultra-light and flexible electromagnetic shielding material, a preparation method and its application, which replaces the traditional conductive fillers of metal particles or metal-coated hollow glass microspheres, and proposes a simple compounding and preparation process, in order to obtain an ultra-light and high-performance electromagnetic shielding material.

[0011] To this end, the specific technical solution adopted by the present invention is as follows:

[0012] According to one aspect of the present invention, a novel ultra-light and flexible electromagnetic shielding material is provided. The novel ultra-light and flexible electromagnetic shielding material is formed by uniformly mixing a matrix and a filler;

[0013] The matrix is ​​composed of the following raw materials in parts by weight: 10 to 20 parts of silicone rubber; 30 to 60 parts of xylene solvent; 30 to 50 parts of cobalt sulfate; 0.5 to 1.0 parts of curing agent;

[0014] The filler is composed of the following raw materials in parts by weight: 10-20 parts of hollow glass microspheres; 5-10 parts of conductive polymer nanomaterials; 1-5 parts of ZrO2-doped TiO2 composite nanoparticles; 2-3 parts of oxidant; and 3-5 parts of carbon aerogel.

[0015] Due to the doping of ZrO2, the light response range of TiO2 is expanded, making it catalytically active under visible light, which helps to improve the electromagnetic shielding effectiveness of the material under light conditions; in addition, under the irradiation of light, ZrO2-doped TiO2 composite nanoparticles can catalyze chemical reactions, such as decomposition of organic pollutants, redox reactions, etc., thereby improving the environmental purification ability of the material.

[0016] According to another aspect of the present invention, a method for preparing a novel ultra-light and flexible electromagnetic shielding material is provided, the method comprising the following steps:

[0017] S1, pre-treating the hollow glass microspheres to obtain hollow glass microspheres with surface amino treatment; activating the carbon aerogel to obtain surface activated carbon aerogel powder;

[0018] S2, coating the surface of the hollow glass microspheres with a conductive polymer nanomaterial, and subjecting the activated carbon aerogel powder to a chemical plating treatment in a cobalt sulfate plating solution (pH value is 6-11) to obtain a cobalt-coated carbon aerogel powder;

[0019] S3, uniformly dispersing ZrO2-doped TiO2 composite nanoparticles on the surface of hollow glass microspheres and carbon aerogel to obtain composite powder;

[0020] S4. Dissolve the silicone rubber in xylene solvent to obtain a silicone rubber solution, add the composite powder and metal particles, add a curing agent after ultrasonic dispersion, and obtain the novel ultra-light and flexible electromagnetic shielding material by tape casting.

[0021] Furthermore, the pretreatment of the hollow glass microspheres includes flotation treatment, hydroxylation treatment and amination treatment;

[0022] The flotation treatment comprises the following steps: weighing a preset weight of hollow glass microbeads, placing them in a deionized water solution, and magnetically stirring them at room temperature until the solution is milky white, then ultrasonically treating them, washing and filtering them with water, and drying them in an oven to obtain the hollow glass microbeads after flotation;

[0023] The hydroxylation treatment comprises the following steps: preparing a NaOH solution of a preset concentration, and placing the hollow glass microspheres after flotation in the NaOH solution to obtain a first mixed solution; placing the first mixed solution in a water bath, and refluxing and stirring at a preset temperature until the reaction is complete, and then standing the first mixed solution at room temperature for a preset time until solid-liquid separation; washing with deionized water to neutrality after flotation, filtering and drying in an oven to obtain hydroxylated hollow glass microspheres;

[0024] The amination treatment comprises the following steps: mixing ethanol and deionized water to obtain an ethanol solution, taking a preset mass of silane coupling agent KH550 with a pipette and adding it to the ethanol solution, stirring evenly to obtain an activation solution; weighing a preset mass of hydroxylated hollow glass microbeads and placing them in the activation solution, and stirring them in a water bath by reflux machinery until the reaction is complete; standing at room temperature for a preset time after the stirring is completed, washing with deionized water to neutrality after flotation, filtering and drying in an oven to obtain the amination hollow glass microbeads.

[0025] Furthermore, the activation treatment of the carbon aerogel to obtain surface-activated carbon aerogel powder includes the following steps: adding palladium chloride to an ethanol solution, heating in a water bath to obtain an activation solution, weighing a preset weight of carbon aerogel and placing it in the activation solution, mechanically stirring, filtering and drying to obtain surface-activated carbon aerogel powder.

[0026] Furthermore, in the flotation treatment step, the concentration of the hollow glass microspheres in the deionized water solution is 0.05-0.07 g / mL, the stirring time is 10-30 min, the ultrasonic time is 10-30 min, and the drying time in the oven is 6-10 h; in the hydroxylation treatment step, the concentration of the NaOH solution is 0.5-1.5 mol / L, the mass ratio of the hollow glass microspheres to the NaOH solution is 3-7%, the reaction temperature is 40-60°C, the stirring speed is 300-500 r / min, the reaction time is 1-3 h, the solution is allowed to stand for 20-40 min, and the drying time in the oven is 6-10 h; amino In the amination step, the mass ratio of ethanol to deionized water is 20-40%, the chemical composition of the silane coupling agent is γ-aminopropyltriethoxysilane, and the mass ratio of the silane coupling agent to the hollow glass microspheres is 5-10%; in the amination step, the reaction temperature is 50-80°C, the stirring speed is 300-500r / min, the reaction time is 1-3h, the solution standing time is 20-40min, and the drying time in the oven is 6-10h; in the activation step, the concentration of the carbon aerosol powder in the activation solution is 0.005-0.01g / mL, the stirring time is 5-30min, and the stirring speed is 400r / min.

[0027] Furthermore, the method of coating the surface of the hollow glass microspheres with the conductive polymer nanomaterial comprises the following steps: preparing a 5-sulfosalicylic acid solution, an ethanol solution and a conductive polymer nanomaterial solution of preset concentrations, mixing them to obtain a polymerization stock solution; weighing a preset mass of the aminated hollow glass microspheres and placing them in the polymerization stock solution, and mechanically stirring them in an ice-water bath until the components are evenly mixed, then adding the FeCl3 solution, and standing at room temperature for a preset time after the reaction is completed; washing with deionized water until neutral after flotation, filtering and drying in an oven to obtain hollow glass microspheres coated with high conductive nanomaterials.

[0028] Furthermore, during the coating reaction, the dopant is a 5-sulfosalicylic acid solution with a concentration of 1 to 1.5 mol / L, the oxidant is a ferric chloride solution with a concentration of 1 to 1.5 mol / L, the mass ratio of ethanol to deionized water is 8 to 15%, the mass ratio of the conductive polymer nanomaterial to the aminated hollow glass microspheres is 1:0.5 to 2.0, the reaction temperature is 0 to 5°C, and the reaction time is 1 to 3 hours. During the in-situ polymerization reaction, the mechanical stirring speed is 300 to 500 r / min, the solution is left to stand for 20 to 40 minutes, and the drying time in the oven is 6 to 10 hours.

[0029] Furthermore, in step S4, the mass ratio of xylene to liquid silicone rubber is 1-4%, the added amount of modified hollow glass microspheres is 4-20%, the added amount of cobalt-plated aerogel is 4-10%, and the added amount of ZrO2-doped TiO2 composite nanoparticles is 1-5%; the ultrasonic time in step S4 is 10-30 minutes, and the curing agent components mainly include tetraethyl orthosilicate and organic tin, and the ratio is 1-4% of the liquid silicone rubber.

[0030] According to another aspect of the present invention, there is provided an application of the above-mentioned new ultra-light flexible electromagnetic shielding material or the new ultra-light flexible electromagnetic shielding material prepared by the preparation method of the new ultra-light flexible electromagnetic shielding material in industrial and commercial electronic products.

[0031] The beneficial effects of the present invention are:

[0032] 1) The hollow glass microspheres of the present invention have a thin-walled hollow structure and a relatively low density. A layer of conductive polymer nanomaterial is coated on the surface thereof by chemical oxidation polymerization to make it conductive and improve the interface bonding between the hollow glass microspheres and the silicone rubber matrix.

[0033] 2) The present invention adopts conductive polymer nanoparticles and metallized aerogel-coated hollow glass microspheres to replace traditional metal particles or metal-coated hollow glass microspheres as silicone rubber fillers. Not only can the two fillers promote each other to be evenly dispersed in the silicone rubber matrix to construct micro-conductive channels, and achieve dielectric parameter regulation and strengthening and shielding performance enhancement, but also can ensure high electromagnetic shielding effectiveness while effectively reducing the density of the composite material and having good flexibility; at the same time, xylene solvent can be used to effectively solve the problem of abnormal breakage of hollow glass microspheres and silicone rubber during the mixing process.

[0034] 3) The present invention adds ZrO2-doped TiO2 composite nanoparticles to the electromagnetic shielding material, which can not only enhance the electromagnetic shielding effectiveness of the material, but also improve the photocatalytic activity, decompose organic pollutants, redox reactions, etc., thereby improving the self-cleaning and antibacterial properties of the material under light conditions, and further significantly improve the comprehensive performance of the ultra-light and flexible electromagnetic shielding material.

[0035] 4) The preparation method of the present invention is simple, and the density of the prepared electromagnetic shielding material is 0.4-0.8 g / cm 3 The electromagnetic shielding effectiveness can reach 30-60dB and can be used in general industrial and commercial electronic products. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 It is a schematic diagram of the principle of a method for preparing a novel ultra-light and flexible electromagnetic shielding material according to an embodiment of the present invention;

[0038] Figure 2 This is a schematic diagram of the microscopic morphology of the hollow glass microspheres directly mixed with silicone rubber in the present invention;

[0039] Figure 3 This is a physical picture of the electromagnetic shielding material of the present invention;

[0040] Figure 4 This is a scanning electron microscope image of the surface of the hollow glass microspheres coated with conductive polymer nanomaterials in the present invention;

[0041] Figure 5 It is a density data diagram of the low-density electromagnetic shielding material prepared by the present invention. DETAILED DESCRIPTION

[0042] To further illustrate each embodiment, the present invention provides drawings, which are part of the disclosure of the present invention and are mainly used to illustrate the embodiments and can be used in conjunction with the relevant descriptions in the specification to explain the operating principles of the embodiments. With reference to these contents, ordinary technicians in the field should be able to understand other possible implementations and advantages of the present invention. The components in the figures are not drawn to scale, and similar component symbols are generally used to represent similar components.

[0043] Example 1

[0044] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, such as Figure 1 As shown, the details are as follows:

[0045] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 50° C. for 2 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0046] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 80°C for 2 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0047] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1.5 mol / L 5-sulfosalicylic acid solution, add 1 ml of polymer nanomaterial monomer dropwise, and finally add 50 ml of 1 mol / L ferric chloride solution. Stir for 3 h in an ice-water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with conductive polymer nanomaterials.

[0048] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 60° C. for 30 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0049] (5) 1 g of activated carbon aerogel was placed in 100 ml of cobalt-containing plating solution with a pH of 8, heated in a water bath at 80° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0050] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0051] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with conductive polymer materials, 0.23 g of cobalt-plated carbon aerogel, and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 20 min, and then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width, and thickness of 22.9 mm, 10.2 mm, and 2 mm, respectively, was demolded.

[0052] It should be noted that the present invention uses silicone rubber and xylene mixed before adding hollow glass microspheres to avoid the problem of hollow glass microspheres breaking. Figure 2 This is the SEM image of the sample obtained by directly mixing the hollow glass microspheres with silicone rubber without adding xylene. It can be seen that the hollow glass microspheres have obvious breakage problems.

[0053] in addition, Figure 3 (In the figure, a represents the front side, and b represents the side bend) is a real picture of the electromagnetic shielding material after the hollow glass microbeads in this example are filled with silicone rubber, showing certain flexibility characteristics.

[0054] Example 2

[0055] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0056] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 40° C. for 1.5 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0057] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 70°C for 3 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0058] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1 mol / L 5-sulfosalicylic acid solution, add 2 ml of polymer nanomaterial monomer dropwise, and finally add 50 ml of 1 mol / L ferric chloride solution. Stir for 2 h in an ice water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with conductive polymer nanomaterials. Figure 4 This is a scanning electron microscope image of the surface of hollow glass microspheres coated with polymer nanomaterials.

[0059] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 50° C. for 40 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0060] (5) 1 g of activated carbon aerogel was placed in 100 ml of cobalt-containing plating solution with a pH of 7, heated in a water bath at 70° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0061] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0062] (6) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with conductive polymer nanomaterials, 0.23 g of cobalt-plated carbon aerogel, and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 15 min, and then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width, and thickness of 30 mm, 20 mm, and 2 mm was demolded.

[0063] Example 3

[0064] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0065] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 50° C. for 2.5 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0066] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 2 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 80°C for 2 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0067] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1.5 mol / L 5-sulfosalicylic acid solution, add 3 ml of polymer nanomaterial monomer dropwise, and finally add 50 ml of 1.5 mol / L ferric chloride solution. Stir for 2 h in an ice water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with conductive polymer nanomaterials.

[0068] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 60° C. for 30 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0069] (5) 1 g of activated carbon aerogel was placed in 100 ml of cobalt-containing plating solution with a pH of 11, heated in a water bath at 90° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0070] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0071] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with conductive polymer nanomaterials and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 15 min, and then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width and thickness of 30 mm, 20 mm and 2 mm was demolded.

[0072] Example 4

[0073] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0074] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 60° C. for 3 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0075] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 60°C for 3 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0076] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1.5 mol / L 5-sulfosalicylic acid solution, add 4 ml of nanomaterial monomer dropwise, and finally add 50 ml of 1.5 mol / L ferric chloride solution. Stir for 3 hours in an ice water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with conductive polymer nanomaterials.

[0077] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 60° C. for 50 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0078] (5) 2 g of activated carbon aerogel was placed in 200 ml of a cobalt-containing plating solution with a pH of 9, heated in a water bath at 70° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0079] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0080] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with polymer nanomaterials and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 25 min, and then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width and thickness of 30 mm, 20 mm and 2 mm was demolded. Figure 4 This is a density data diagram of the low-density electromagnetic shielding material prepared by the present invention.

[0081] Example 5

[0082] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0083] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 50° C. for 2 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0084] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 80°C for 2 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0085] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1 mol / L 5-sulfosalicylic acid solution, add 4 ml of nanomaterial monomer dropwise, and finally add 50 ml of 1 mol / L ferric chloride solution. Stir for 2 h in an ice-water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with conductive polymer nanomaterials.

[0086] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 70° C. for 30 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0087] (5) 1 g of activated carbon aerogel was placed in 100 ml of a cobalt-containing plating solution with a pH of 9, heated in a water bath at 80° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0088] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0089] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.95 g of hollow glass microspheres coated with polymer nanomaterials and 0.35 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 20 min, and then a certain amount of curing agent (4% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width and thickness of 30 mm, 20 mm and 2 mm was demolded.

[0090] Example 6

[0091] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0092] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 50° C. for 2 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0093] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 80°C for 2 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0094] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1 mol / L 5-sulfosalicylic acid solution, add 4 ml of polymer nanomaterial monomer dropwise, and finally add 50 ml of 1 mol / L ferric chloride solution. Stir for 2 h in an ice water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with polyconductive polymer nanomaterials.

[0095] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 70° C. for 30 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0096] (5) 1 g of activated carbon aerogel was placed in 100 ml of cobalt-containing plating solution with a pH of 10, heated in a water bath at 80° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0097] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0098] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with polymer nanomaterials, 0.5 g of nickel powder, and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 20 min, and then a certain amount of curing agent (4% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width, and thickness of 30 mm, 20 mm, and 2 mm was demolded.

[0099] Example 7

[0100] A method for preparing a novel ultra-light and flexible electromagnetic shielding material, comprising:

[0101] (1) First, 10 g of hollow glass microspheres were floated with a deionized water solution at room temperature, then placed in a NaOH solution, refluxed and stirred in a water bath at 50° C. for 2 h, washed with deionized water until neutral after flotation, filtered and dried to obtain hydroxylated microspheres.

[0102] (2) 10 g of hydroxylated microbeads were placed in a mixed solution of ethanol and deionized water in a mass ratio of 3:1, 1 g of silane coupling agent KH550 was added, and the mixture was refluxed and stirred in a water bath at 80°C for 2 h. After flotation, the mixture was washed with deionized water until neutral, filtered and dried to obtain amino microbeads.

[0103] (3) Take 2 g of amino microbeads and place them in a mixed solution of 400 ml of ethanol and deionized water in a mass ratio of 10:1, add 50 ml of 1 mol / L 5-sulfosalicylic acid solution, add 4 ml of nanomaterial monomer dropwise, and finally add 50 ml of 1 mol / L ferric chloride solution. Stir for 2 h in an ice-water bath, wash with deionized water until neutral after flotation, filter and dry to obtain hollow glass microbeads coated with polymer nanomaterials.

[0104] (4) 10 g of carbon aerogel powder was placed in a water bath heated at 60° C. for 30 min and then 0.1 g of palladium chloride was added to 1000 ml of 10% ethanol solution to obtain activated carbon aerogel.

[0105] (5) 1 g of activated carbon aerogel was placed in 100 ml of cobalt-containing plating solution with a pH of 8, heated in a water bath at 70° C. for 1 h, and filtered and dried to obtain cobalt-coated carbon aerogel powder.

[0106] (6) Dissolve 5 g of titanate (such as titanium tetrachloride) and 1.5 g of zirconol (such as zirconium isopropoxide) in 9 ml of ethanol solution, use hydrochloric acid to adjust the pH value of the solution to 1-2, stir evenly at room temperature for 1 hour, let the stirred solution stand for 24 hours to form a gel, age the gel at room temperature for 72 hours, dry it in an oven at 60°C for 24 hours to obtain a dry gel, put the dried gel into an oven, and calcine it at 300°C for 2 hours, grind the calcined sample into fine powder using a grinding equipment, sieve the ground powder using a 200-mesh sieve to obtain ZrO2-doped TiO2 composite nanoparticles.

[0107] (7) 1 g of liquid silicone rubber and 3 g of xylene were mixed and fully dissolved, and 0.76 g of hollow glass microspheres coated with polymer nanomaterials, 0.5 g of cobalt powder, and 0.25 g of ZrO2-doped TiO2 composite nanoparticles were added. Ultrasonic dispersion was performed for 20 min, and then a certain amount of curing agent (4% of the liquid silicone rubber) was added dropwise. After stirring evenly, the solution was immediately poured onto the mold. After standing and curing for 24 hours, the low-density electromagnetic shielding material with a length, width, and thickness of 30 mm, 20 mm, and 2 mm was demolded.

[0108] Example 8

[0109] This experiment uses a network analyzer to measure the power or phase change of electromagnetic waves after passing through the shielding material, and calculates the electromagnetic shielding effectiveness through the corresponding algorithm. Network analyzers are based on waveguide technology and are divided into scalar network analyzers (SNA) and vector network analyzers (VNA). Compared with SNA, VNA can not only detect power changes, but also analyze complex signals (such as composite dielectric constant and magnetic permeability), and has a wider range of applications. During measurement, VNA transmits electromagnetic waves within the test frequency range from two ports, and simultaneously records the radiation data reflected and transmitted through the shielding material. In a two-port VNA, both the incident wave and the transmitted wave can be digitally represented by S parameters. These S parameters are related to the reflection and transmission of electromagnetic waves, respectively, and the S parameters are specified as four sets of data: forward reflection (S11), reverse reflection (S22), forward transmission (S12), and reverse transmission (S21).

[0110] The calculation of electromagnetic shielding effectiveness depends on the measurement results of S parameters (S11, S22, S12, S21), and the calculation formula is as follows:

[0111] R=|S 11 | 2 (1)

[0112] T=|S 21 | 2 (2)

[0113] R+A+T=1 (3)

[0114]

[0115]

[0116] SE T =SE R +SE A +SE M (dB) (6)

[0117] R, T, A are reflection coefficient, transmission coefficient, and absorption coefficient respectively. T , SE R and SE A They are the total, reflected and absorbed electromagnetic interference shielding effectiveness, SE M is the shielding effectiveness of internal multiple reflections and can usually be ignored.

[0118] Figure 5 This is a density data diagram of the low-density electromagnetic shielding material prepared by the present invention. It can be seen that the density of the electromagnetic shielding composite material obtained by the present invention is relatively low, at 1g / cm 3 the following.

[0119] For the performance test of the existing comparative example, the specific preparation process is described as follows:

[0120] Comparative Example 1

[0121] Mix 1g of liquid silicone rubber and 3g of xylene and fully dissolve them. Then add a certain amount of curing agent (2% of the liquid silicone rubber) and stir evenly. Then pour the solution on the mold immediately. After standing and curing for 24 hours, demold the material to obtain an electromagnetic shielding material with a length, width and thickness of 30mm, 20mm and 2mm respectively.

[0122] Comparative Example 2

[0123] Mix 1g of liquid silicone rubber and 3g of xylene and fully dissolve them, add 0.76g of untreated hollow glass beads, and ultrasonically disperse them for 20 minutes. Then, add a certain amount of curing agent (2% of the liquid silicone rubber). After stirring evenly, pour the solution on the mold immediately. After standing and curing for 24 hours, demold the material to obtain an electromagnetic shielding material with a length, width and thickness of 30mm, 20mm and 2mm respectively.

[0124] Comparative Example 3

[0125] The surface of the hollow glass microspheres was coated with metal nickel by chemical plating to obtain nickel-plated hollow glass microspheres. Then 1g of liquid silicone rubber and 3g of xylene were mixed and fully dissolved, 3.6g of nickel-plated hollow glass microspheres were added, and ultrasonic dispersion was performed for 20 minutes. Then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise, and the solution was immediately poured onto the mold after stirring evenly. After standing and curing for 24 hours, the electromagnetic shielding material with a length, width and thickness of 30mm, 20mm and 2mm was demolded.

[0126] Comparative Example 4

[0127] The metal cobalt was coated on the surface of the hollow glass microspheres by chemical plating to obtain cobalt-plated hollow glass microspheres. Then 1g of liquid silicone rubber and 3g of xylene were mixed and fully dissolved, 3.6g of cobalt-plated hollow glass microspheres were added, ultrasonic dispersion was performed for 20 minutes, and then a certain amount of curing agent (2% of the liquid silicone rubber) was added dropwise, and the solution was immediately poured on the mold after stirring evenly. After standing and curing for 24 hours, the electromagnetic shielding material with a length, width and thickness of 30mm, 20mm and 2mm was demolded.

[0128] Comparative Example 5

[0129] 100 parts by weight of silicone rubber, 5 parts by weight of azodicarbonamide, 4 parts by weight of 2,5-dimethyl-2,5-bishexane, 0.3 parts by weight of diisopropylbenzene peroxide, 4 parts by weight of zinc oxide and 4 parts by weight of stearic acid are fully mixed in an internal mixer, and then 45 parts by weight of highly conductive carbon black and 10 parts by weight of conductive few-layer graphene are added into the internal mixer and mixed to obtain a rubber compound, which is rolled on an open mixer for 25 minutes to discharge bubbles in the rubber compound and cut into sheets of 9 cm×13 cm in size, the temperature of the embedded mold in the vulcanizer is preheated to 180° C., the pressure is set to 10 MPa, and then the sheet is placed on a 15 cm×15 cm glass paper and placed in a vulcanizer for high-temperature curing and foaming for 320 seconds to obtain a foamed silicone rubber composite material for electromagnetic shielding.

[0130] Table 1 lists some existing comparative performance test results, and Table 2 lists the electromagnetic shielding material performance test results of this embodiment.

[0131] Table 1 Comparative Example Electromagnetic Shielding Material Performance Test Results

[0132]

[0133] Table 2 Test results of electromagnetic shielding material performance in the embodiment

[0134]

[0135]

[0136] Table 2 shows the performance test results of the electromagnetic shielding material of this embodiment. The maximum electromagnetic shielding capability reaches 55.8, while the density is only 0.77g / cm3, which is much lower than the density value of electromagnetic shielding in existing literature. Compared with the performance test results of Table 1, the conductive polymer nanomaterial coated hollow glass microsphere material, cobalt-plated aerogel and dispersion method proposed in this patent are simple and have significant performance advantages.

[0137] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A new type of ultra-light and flexible electromagnetic shielding material, characterized in that: The new ultra-light and flexible electromagnetic shielding material is made of a uniform mixture of a matrix and a filler; Wherein, the matrix is ​​composed of the following raw materials in parts by weight: Silicone rubber 10~20 parts; 30-60 parts of xylene solvent; 30-50 parts of cobalt sulfate; Curing agent 0.5~1.0 part; The filler is composed of the following raw materials in parts by weight: 10~20 parts of hollow glass microspheres; 5-10 parts of conductive polymer nanomaterials; 1-5 parts of ZrO2-doped TiO2 composite nanoparticles; 2~3 parts of oxidant; 3~5 parts of carbon aerogel.

2. A method for preparing a novel ultra-light and flexible electromagnetic shielding material, used to prepare the novel ultra-light and flexible electromagnetic shielding material as claimed in claim 1, characterized in that: The preparation method comprises the following steps: S1, pre-treating the hollow glass microspheres to obtain hollow glass microspheres with surface amino treatment; activating the carbon aerogel to obtain surface activated carbon aerogel powder; S2, coating the surface of the hollow glass microspheres with a conductive polymer nanomaterial, and subjecting the activated carbon aerogel powder to a chemical plating treatment in a cobalt sulfate plating solution to obtain a cobalt-coated carbon aerogel powder; S3, uniformly dispersing ZrO2-doped TiO2 composite nanoparticles on the surface of hollow glass microspheres and carbon aerogel to obtain composite powder; S4. Dissolve the silicone rubber in xylene solvent to obtain a silicone rubber solution, add the composite powder and metal particles, add a curing agent after ultrasonic dispersion, and obtain the novel ultra-light and flexible electromagnetic shielding material by tape casting.

3. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 2, characterized in that: The pretreatment of the hollow glass microspheres includes flotation treatment, hydroxylation treatment and amination treatment; Wherein, the flotation process comprises the following steps: Weigh a preset number of hollow glass microbeads by weight, place them in a deionized water solution, and stir them magnetically at room temperature until the solution turns milky white, then perform ultrasonic treatment, wash and filter, and dry them in an oven to obtain the hollow glass microbeads after flotation; The hydroxylation treatment comprises the following steps: A NaOH solution of a preset concentration is prepared, and the hollow glass microspheres after flotation are placed in the NaOH solution to obtain a first mixed solution; the first mixed solution is placed in a water bath, and refluxed and stirred at a preset temperature until the reaction is complete, and then the first mixed solution is allowed to stand at room temperature for a preset time until solid-liquid separation; after flotation, the solution is washed with deionized water until neutral, filtered and dried in an oven to obtain hydroxylated hollow glass microspheres; The amination treatment comprises the following steps: Ethanol and deionized water are mixed to obtain an ethanol solution, and a preset mass of silane coupling agent is taken with a pipette and added to the ethanol solution, and the activation solution is obtained after stirring evenly; a preset mass of hydroxylated hollow glass microbeads are weighed and placed in the activation solution, and mechanically stirred in a water bath by reflux until the reaction is complete; after the stirring is completed, the mixture is allowed to stand for a preset time at room temperature, and after flotation, it is washed with deionized water until neutral, filtered, and dried in an oven to obtain amino hollow glass microbeads.

4. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 3, characterized in that: The activation treatment of the carbon aerogel to obtain the surface activated carbon aerogel powder comprises the following steps: Palladium chloride is added to an ethanol solution, heated in a water bath to obtain an activation solution, and a preset weight portion of carbon aerogel is weighed and placed in the activation solution, mechanically stirred, filtered and then dried to obtain surface-activated carbon aerogel powder.

5. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 4, characterized in that: In the flotation treatment step, the concentration of the hollow glass microspheres in the deionized water solution is 0.05-0.07 g / mL, the stirring time is 10-30 min, the ultrasonic time is 10-30 min, and the drying time in the oven is 6-10 h; In the hydroxylation treatment step, the concentration of NaOH solution is 0.5-1.5 mol / L, the mass ratio of hollow glass microspheres to NaOH solution is 3-7%, the reaction temperature is 40-60°C, the stirring speed is 300-500 r / min, the reaction time is 1-3 h, the solution standing time is 20-40 min, and the drying time in the oven is 6-10 h; In the amination treatment step, the mass ratio of ethanol to deionized water is 20-40%, the chemical composition of the silane coupling agent is γ-aminopropyltriethoxysilane, and the mass ratio of the silane coupling agent to the hollow glass microspheres is 5-10%; In the amination step, the reaction temperature is 50-80°C, the stirring speed is 300-500 r / min, the reaction time is 1-3 hours, the solution standing time is 20-40 minutes, and the drying time in the oven is 6-10 hours; In the activation treatment step, the concentration of the carbon aerosol powder in the activation solution is 0.005-0.01 g / mL, the stirring time is 5-30 min, and the stirring speed is 400 r / min.

6. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 2, characterized in that: The method of coating the conductive polymer nanomaterial on the surface of the hollow glass microspheres comprises the following steps: Preparing a 5-sulfosalicylic acid solution, an ethanol solution and a conductive polymer nanomaterial solution of preset concentrations, and mixing them to obtain a polymerization stock solution; Weigh a preset mass of aminated hollow glass microspheres and place them in the polymerization stock solution, and mechanically stir them in an ice-water bath until the components are evenly mixed, then add FeCl3 solution, and let stand at room temperature for a preset time after the reaction is completed; After flotation, the product is washed with deionized water until it becomes neutral, filtered and dried in an oven to obtain hollow glass microbeads coated with highly conductive nanomaterials.

7. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 6, characterized in that: During the coating reaction, the dopant is a 5-sulfosalicylic acid solution with a concentration of 1~1.5 mol / L, the oxidant is a ferric chloride solution with a concentration of 1~1.5 mol / L, the mass ratio of ethanol to deionized water is 8~15%, the mass ratio of the conductive polymer nanomaterial to the amino hollow glass microspheres is 1:0.5~2.0, the reaction temperature is 0~5°C, and the reaction time is 1~3h.

8. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 6, characterized in that: During the in-situ polymerization reaction, the mechanical stirring speed is 300~500r / min, the solution is allowed to stand for 20~40min, and the drying time in the oven is 6~10h.

9. The method for preparing a novel ultra-light and flexible electromagnetic shielding material according to claim 2, characterized in that: In step S4, the mass ratio of xylene to liquid silicone rubber is 1-4%, the addition amount of modified hollow glass microspheres is 4-20%, the addition amount of cobalt-plated aerogel is 4-10%, and the addition amount of ZrO2-doped TiO2 composite nanoparticles is 1-5%; In step S4, the ultrasonic time is 10-30 minutes, and the curing agent components mainly include ethyl orthosilicate and organic tin, and the ratio is 1-4% of the liquid silicone rubber.

10. Application of the new ultra-light and flexible electromagnetic shielding material described in claim 1 or the new ultra-light and flexible electromagnetic shielding material prepared by the preparation method of any one of claims 2 to 9 in industrial and commercial electronic products.

Citation Information

Patent Citations

  • Hollow multilayer core-shell material with electromagnetic wave adsorption characteristic and preparation method thereof

    CN102504758A

  • Preparation method of nano TiO2 / ZrO2 composite catalyst

    CN110586058A

  • Low-thermal-conductivity electromagnetic shielding polyimide-based composite material and preparation method thereof

    CN114539572A

  • Modified PBT material and preparation method thereof

    CN115403899A

  • Method for synthesizing polyurethane coating of shielding film of electronic product

    CN115820093A

Cited By

  • Silicone rubber hollow glass bead composite electromagnetic shielding material and preparation method thereof

    CN121038254A