P-ni3inc0.7 nanomaterial with porous fibrous structure and preparation method and application thereof

Porous fibrous p-Ni3InC0.7 nanomaterials were prepared by electrospinning and high-temperature zinc evaporation, which solved the problems of low specific surface area and poor conductivity of perovskite-based electrocatalysts and achieved low-cost and high-efficiency improvement in electrocatalytic water oxidation performance.

CN117867693BActive Publication Date: 2026-11-10HUAZHONG UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410004592.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-03
Publication Date
2026-11-10
Estimated Expiration
2044-01-03

AI Technical Summary

Technical Problem

Existing perovskite-based electrocatalysts suffer from high initial OER potential, low specific surface area, and poor conductivity during water electrolysis for hydrogen production. Traditional preparation methods are complex and costly, resulting in low catalytic stability and efficiency.

Method used

Porous fibrous p-Ni3InC0.7 nanomaterials were prepared by electrospinning and high-temperature zinc element evaporation. The pore size was controlled by adjusting the zinc content, thereby increasing the specific surface area and optimizing the catalytic active sites. An environmentally friendly preparation process was used to replace the precious metal catalyst.

Benefits of technology

This method enables the efficient and low-cost large-scale preparation of electrode materials, improves the catalytic performance and stability of the catalyst, exposes more active sites, and enhances the efficiency of electrocatalytic water oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117867693B_ABST
    Figure CN117867693B_ABST
Patent Text Reader

Abstract

This invention discloses a p-Ni3InC with a porous fibrous structure. 0.7 Nanomaterials and their preparation methods belong to the field of electrocatalytic electrode material preparation technology and can be used for electrocatalytic OER reactions. An indium source, a nickel source, zinc nitrate hexahydrate, polyacrylonitrile (PAN) with a molecular weight of 150,000, and N,N-dimethylformamide are mixed and stirred overnight at room temperature to form a homogeneous solution. The resulting solution is then added to an electrospinning system, and a high voltage is applied to form a fibrous film, which is dried overnight. The film is then annealed in a tube furnace to obtain black p-Ni3InC. 0.7 Nanomaterials. This invention prepares porous fibrous anti-perovskite carbide nanomaterials via electrospinning and zinc elemental evaporation. These materials exhibit good activity in OER reactions and low cost, demonstrating significant commercial potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalytic electrode material preparation technology, specifically relating to a p-Ni3InC electrode with a porous fibrous structure. 0.7 Preparation method of nanomaterials and the obtained p-Ni3InC 0.7 Nanomaterials can serve as highly efficient catalysts for water oxidation. Background Technology

[0002] With global restrictions on carbon emissions and national-level "carbon peaking" and "carbon neutrality" strategies, changing the current energy structure and increasing the proportion of renewable energy is particularly important. A promising alternative to fossil fuels is green hydrogen, which can be produced through the electrolysis of water using renewable electricity. Developing and utilizing hydrogen energy from renewable energy sources has become an important global development direction. Due to its zero-pollution, high efficiency, abundant sources, and wide range of applications, many countries with severe environmental pollution regard hydrogen energy as a future energy source. Currently, there are three main methods for hydrogen production: steam methane reforming, coal gasification, and water electrolysis. Among these, water electrolysis has unparalleled advantages over other methods, as its raw material is abundant water, and the entire process does not produce any harmful gases or waste liquids.

[0003] When an electric current flows through the electrolyte to form a circuit, water molecules decompose into hydrogen and oxygen. Theoretically, this involves two half-reactions. When a polarizing current is applied, negatively charged hydroxide ions accumulate near the anode, where they are oxidized to release oxygen, resulting in the oxygen evolution reaction (OER). Conversely, positively charged hydrogen ions accumulate near the cathode, where they are reduced to produce hydrogen gas, resulting in the hydrogen evolution reaction (HER). The reaction equations under different conditions are as follows:

[0004] Overall reaction:

[0005] H2O→H2+1 / 2O2

[0006] In acidic solution:

[0007] Cathode 2H + +2e - →H2

[0008] Anode H2O→2H + +1 / 2O2+2e -

[0009] In neutral and alkaline solutions:

[0010] cathode 2H2O + 2e - →H2+2OH -

[0011] Anode 2OH - →H₂O + 1 / 2O₂ + 2e-

[0012] The perovskite family, as a vast family of crystalline materials, has attracted extensive research in academia due to its wide range of functions and underlying reaction mechanisms. However, in the field of electrocatalysis, it suffers from drawbacks such as high initial potential of OER (Optical Emission Reduction), low specific surface area, and poor conductivity. In contrast, anti-perovskites, which share a similar cubic structure with perovskites, not only possess the advantages of flexible and tunable perovskite composition but also overcome the disadvantages of poor conductivity. Anti-perovskites are a crystal structure resulting from the inversion of perovskite cations and anions. Due to the cation-rich sites at the face centers of the cubic crystal, they exhibit unconventional physical and chemical properties. However, traditional anti-perovskite preparation methods are limited, and most lack desirable morphologies. Therefore, improving the preparation process from the source is highly promising. Summary of the Invention

[0013] In view of this, the object of the present invention is to provide an anti-perovskite p-Ni3InC with a porous fibrous structure. 0.7 The present invention discloses a method for preparing nanomaterials using nickel-based materials and polyacrylonitrile as a carbon source to prepare anti-perovskite carbides. This method solves the technical problems of complex preparation processes, high costs, low efficiency, and poor catalytic stability in current technologies, and can improve the catalytic performance of nickel-based catalysts. The invention also optimizes the porous structure to further ensure the improvement of catalyst performance.

[0014] To achieve the above objectives, the present invention adopts the following technical solution:

[0015] The first technical objective of this invention is to provide a p-Ni3InC with a porous fibrous structure. 0.7 The preparation method of nanomaterials includes the following steps:

[0016] (1) Preparation of polymer solution: Indium source, nickel source, zinc nitrate hexahydrate and polyacrylonitrile are added to N,N dimethylformamide solution and stirred thoroughly overnight to obtain a homogeneous solution;

[0017] (2) Preparation of fibrous nanomaterials: The solution from step (1) was injected into a 10 mL disposable syringe and placed in a high-voltage electrospinning device. The white thin film product was collected using a roller device.

[0018] (3) Preparation of porous fibrous p-Ni3InC 0.7 Nanomaterials: The thin film product collected in step (2) was annealed and then naturally cooled and ground to obtain a black powder p-Ni3InC. 0.7 Nanomaterials.

[0019] It should be noted that this invention prepares porous fiber structure nanomaterials by electrospinning and high-temperature zinc element evaporation. The zinc content can be adjusted to regulate the pore size, optimize the specific surface area, and thus improve the catalytic kinetics. This is a simple, efficient, and environmentally friendly method that can be used to replace precious metal catalysts for the large-scale preparation of electrode materials.

[0020] Optionally, in step (1), the molar ratio of the indium source, nickel source, and zinc nitrate hexahydrate is 1:3:(1-3); the weight-average molecular weight M of the polyacrylonitrile is... W The value is 150,000, and the ratio of polyacrylonitrile to N,N-dimethylformamide is 0.63 g: 5 mL.

[0021] Further, in step (1), the indium source is indium nitrate, and the nickel source is nickel acetate, nickel nitrate, or nickel chloride; the stirring speed is 500 r / min, and the stirring time is 12 h.

[0022] Optionally, in step (2), in the electrospinning system, the roller collector is 16-20 cm away from the needle tip, the needle type is 23-G, the working voltage is 16-20 kV, the syringe pusher speed is 0.3-0.6 mL / h, and the temperature is 20-25 °C.

[0023] Optionally, in step (3), the annealing process is performed as follows:

[0024] The thin film product collected in step (2) was placed in a tube furnace and heated to 850-900°C at a rate of 5°C / min under an inert atmosphere and maintained for 2-3 hours.

[0025] The second technical objective of this invention is to provide a p-Ni3InC with a porous fibrous structure prepared by the method described above. 0.7 Nanomaterials.

[0026] The third technical objective of this invention is to provide a p-Ni3InC with a porous fibrous structure prepared by the method described above. 0.7 Applications of nanomaterials in electrocatalysis.

[0027] Furthermore, the p-Ni3InC with a porous fibrous structure 0.7 Application of nanomaterials as catalysts for electrocatalytic water oxidation.

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] (1) This invention uses electrospinning to prepare nickel-based anti-perovskite, which, compared to nanomaterials prepared by traditional hydrothermal methods, has a larger specific surface area and exposes more active sites, thereby improving catalytic reaction kinetics. This invention provides a practically feasible p-Ni3InC 0.7 The preparation methods for nanomaterials are not only inexpensive and pollution-free, but also have great commercial potential.

[0030] (2) This invention employs a zinc element evaporation method, utilizing the physical property that zinc evaporates at high temperatures to form pores in the fiber structure. By adjusting the zinc source content, the size of the pores can be adjusted, thereby regulating the specific surface area and further enhancing the catalytic activity. When the zinc source is 0.75 mmol, the pores are most uniform and suitable.

[0031] In summary, this invention employs a simple electrospinning and high-temperature calcination method to prepare multi-fibrous anti-perovskite catalysts to enhance catalytic activity and stability. It also provides a method for preparing porous fiber structure catalysts, which is a simple, non-polluting method for large-scale preparation of electrode materials. Attached Figure Description

[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.

[0033] Figure 1 It is the porous fibrous structure of p-Ni3InC described in this invention. 0.7 A schematic diagram of the preparation process of nanomaterials.

[0034] Figure 2 The porous fibrous structure p-Ni3InC prepared in Example 1 and Comparative Example 1 of this invention is... 0.7 Nanomaterials and Ni3InC prepared by hydrothermal method 0.7 XRD patterns.

[0035] Figure 3 The fibrous p-Ni3InC prepared in Comparative Example 1 of this invention 0.7 SEM image of nanomaterials.

[0036] Figure 4 The porous fibrous structure p-Ni3InC prepared in Example 2 of this invention 0.7 SEM image of nanomaterials.

[0037] Figure 5The porous fibrous structure p-Ni3InC prepared in Example 1 of this invention 0.7 SEM image of nanomaterials.

[0038] Figure 6 The porous fibrous p-Ni3InC structures prepared in Example 1 and Comparative Example 1 of this invention are 0.7 BET comparison chart of nanomaterials.

[0039] Figure 7 The porous fibrous p-Ni3InC structures prepared in Example 1 and Comparative Example 1 of this invention are 0.7 Comparison of the catalytic performance of nanomaterials. Detailed Implementation

[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0041] The term "embodiment" used herein, as an example, is not necessarily to be construed as superior to or better than other embodiments. Performance testing in the embodiments of this application, unless otherwise specified, employs conventional testing methods in the art. It should be understood that the terminology used in this application is merely for describing particular implementations and is not intended to limit the scope of this disclosure.

[0042] Unless otherwise stated, the technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; other experimental methods and technical means not specifically mentioned herein refer to experimental methods and technical means commonly used by one of ordinary skill in the art.

[0043] To better illustrate the content of this application, numerous specific details are provided in the following detailed embodiments. Those skilled in the art should understand that this application can be implemented even without certain specific details. In the embodiments, some methods, means, instruments, and devices well-known to those skilled in the art are not described in detail in order to highlight the main points of this application.

[0044] Without conflict, the technical features disclosed in the embodiments of this application can be combined arbitrarily, and the resulting technical solution belongs to the content disclosed in the embodiments of this application.

[0045] This invention provides a p-Ni3InC with a porous fibrous structure. 0.7The preparation method of nanomaterials uses electrospinning and high-temperature annealing to prepare catalysts with porous fibrous structures, thereby improving the catalytic performance of the catalysts.

[0046] To better understand the present invention, the following embodiments are provided for further detailed description of the present invention, but they should not be construed as limiting the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above-described invention are also considered to fall within the protection scope of the present invention.

[0047] Example 1

[0048] A p-Ni3InC with a porous fibrous structure 0.7 The preparation method of nanomaterials includes the following steps:

[0049] (1) Preparation of polymer precursor solution: Dissolve 0.25 mmol indium nitrate 4.5 hydrate, 0.75 mmol nickel acetate, 0.75 mmol zinc nitrate hexahydrate and 0.6 g polyacrylonitrile in 5 mL LMF solution, stir thoroughly at 500 r / min for 12 h to form a uniform precursor solution with a certain viscosity.

[0050] (2) Preparation of fibrous nanostructures: The solution obtained in step (1) was transferred to a 10 mL syringe with a G-23 needle, a voltage of 18 kV, and a syringe injection rate of 0.3 mL / h. The product was collected using a roller collector with the needle tip 16 cm from the substrate.

[0051] (3) Preparation of porous fibrous nanomaterials: The film on the drum collector in step (2) is placed in a tube furnace and annealed at high temperature in an inert gas atmosphere at 900℃, with a heating rate of 5℃ / min and a holding time of 3h to evaporate the zinc element. After cooling, the film is ground to obtain a black powder, which is p-Ni3InC. 0.7 Nanomaterials.

[0052] To further demonstrate the beneficial effects of the present invention and to better understand it, the technical features disclosed in the present invention are further illustrated by the following comparative examples, but these should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above description of the invention, without inventive effort, are also considered to fall within the protection scope of the present invention.

[0053] Example 2

[0054] The difference between Example 2 and Example 1 is that the amount of zinc nitrate added is 0.25 mmol, and the ratio of zinc nitrate to indium is 1:1.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that zinc was not added in step (1), while the other parameters and specific implementation steps are the same as in Example 1.

[0057] Figure 1 To prepare porous fibrous p-Ni3InC 0.7 The process flow diagram for nanomaterials is as follows: First, a polymer precursor solution is prepared, and then a fibrous precursor structure is fabricated using electrospinning. The main principle is that charged polymers are accelerated at the apex of the Taylor cone of a capillary under high voltage. When the voltage is high enough, the polymer overcomes surface tension to form a jet stream. During the jetting process, the solution evaporates or solidifies and eventually falls onto a receiving device, forming a fibrous material structure. Furthermore, sufficient stirring is necessary to ensure a more uniform ionic polymer in the solution, which is beneficial for the formation of uniform pores in the next step. Different amounts of zinc can yield porous nanostructures of different sizes.

[0058] Figure 2 Ni3InC prepared by hydrothermal method in Example 1 and Comparative Example 1 0.7 The XRD pattern shows a series of characteristic peaks at 23.5°, 33.5°, 41.3°, 48.1°, 54.2°, 59.8°, 70.3°, and 75.3°, corresponding to its (100), (110), (111), (200), (210), (211), (220), and (221) crystal planes, respectively. Furthermore, in p-Ni3InC... 0.7 In the spectrum, a graphitic carbon peak was observed at 25.7°, which is attributed to the partial bonding of polyacrylonitrile in the polymer solution with metal ions to form products at high temperature, and the partial formation of graphitic carbon.

[0059] Figure 3 Fiber-like p-Ni3InC prepared for Comparative Example 1 0.7 SEM morphology of nanomaterials.

[0060] Figure 4 The porous fibrous structure p-Ni3InC prepared in Example 2 0.7 SEM image of the nanomaterial shows that the fibrous structure has many collapses and uneven pores.

[0061] Figure 5 The porous fibrous structure p-Ni3InC prepared in Example 1 0.7 SEM morphology of the nanomaterial. Compared with Comparative Example 1, a clear contrast in pores can be seen. When the temperature reaches the evaporation temperature of zinc, zinc is evaporated and forms a pore structure on the fiber structure. The pore structure is related to factors such as stirring time, zinc content, and annealing temperature.

[0062] Figure 6 The porous fibrous p-Ni3InC structures prepared in Example 1 and Comparative Example 1 0.7 BET comparison chart of nanomaterials. It can be clearly seen that due to the presence of pores, p-Ni3InC... 0.7 The specific surface area has been greatly increased, thus exposing more active sites.

[0063] Figure 7 The porous fibrous p-Ni3InC structures prepared in Example 1 and Comparative Example 1 0.7 The comparison chart of the catalytic performance of nanomaterials shows that the porous structure of nanomaterials has a significant improvement in performance. Furthermore, a larger nickel oxidation peak can be observed, indicating that the porous material exposes more nickel active sites, which is one of the reasons for the improved catalytic performance.

[0064] Table 1. Porous fibrous p-Ni3InC structures prepared in Example 1 0.7 EDS table of nanomaterials

[0065]

[0066] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A p-Ni3InC with a porous fibrous structure 0.7 The application of nanomaterials in electrocatalysis is characterized by, p-Ni3InC with a porous fibrous structure 0.7 The preparation method of nanomaterials includes the following steps: (1) Preparation of polymer solution: Indium source, nickel source, zinc nitrate hexahydrate and polyacrylonitrile are added to N,N dimethylformamide solution and stirred thoroughly overnight to obtain a homogeneous solution; The molar ratio of the indium source, nickel source and zinc nitrate hexahydrate is 1:3:(1-3); the weight-average molecular weight (MW) of polyacrylonitrile is 150,000, and the molar ratio of polyacrylonitrile to N,N-dimethylformamide is 0.63 g: 5 mL. The indium source is indium nitrate, and the nickel source is nickel acetate, nickel nitrate, or nickel chloride; (2) Preparation of fibrous nanomaterials: The solution from step (1) was injected into a 10 mL disposable syringe and placed in a high-voltage electrospinning device. The white thin film product was collected using a roller device. (3) Preparation of porous fibrous p-Ni3InC 0.7 Nanomaterials: The thin film product collected in step (2) was annealed and then naturally cooled and ground to obtain a black powder p-Ni3InC. 0.7 Nanomaterials; The annealing process is as follows: The thin film product collected in step (2) was placed in a tube furnace and heated to 850-900°C at a rate of 5°C / min under an inert atmosphere and maintained for 2-3 hours.

2. The p-Ni3InC with a porous fibrous structure according to claim 1 0.7 The application of nanomaterials in electrocatalysis is characterized by, In step (1), the stirring speed is 500 r / min and the stirring time is 12 h.

3. The p-Ni3InC with a porous fibrous structure according to claim 1 0.7 The application of nanomaterials in electrocatalysis is characterized by, In step (2), in the electrospinning system, the roller collector is 16-20 cm away from the needle tip, the needle type is 23-G, and the working voltage is 16-20 kV; the syringe pusher speed is 0.3-0.6 mL / h, and the temperature is 20-25℃.

4. The p-Ni3InC with a porous fibrous structure according to claim 1 0.7 The application of nanomaterials in electrocatalysis is characterized by, p-Ni3InC with a porous fibrous structure 0.7 Application of nanomaterials as catalysts for electrocatalytic water oxidation.

Citation Information

Patent Citations

  • Cobalt-nickel alloy / carbon nanofiber composite electrocatalyst, and preparation method and application thereof

    CN111841546A

  • Composite electrocatalyst, preparation method and application thereof