An indoor test method for testing the anti-reflective crack performance of asphalt mixture
Through repeated loading tests of combined test pieces and special fixtures, the problem of high cost of anti-reflection crack performance evaluation of asphalt mixtures in the prior art is solved and the coupling effect of traffic load and temperature stress cannot be simulated, thus achieving low-cost and simple operation of asphalt Evaluation of anti-reflective crack performance of mixes, suitable for pavement material selection and mix optimization.
Patent Information
- Application Number
- CN202410061173.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-16
AI Technical Summary
The indoor test cost of anti-reflection crack performance of existing asphalt mixtures is high and it is impossible to objectively evaluate the suppression ability under the simultaneous coupling of traffic loads and temperature stresses. The existing test methods are complex in operation and cannot simulate the reflection caused by traffic loads and temperature stresses simultaneously. Cracks emerge and develop.
Combined specimens include asphalt mixture specimens and cement concrete specimens. The cement blocks and strain gauge are adhered by heating the melted asphalt adhesive to simulate semi-rigid base cracks, and repeated loading tests are carried out in combination with special specimen fixtures. The strain gauge resistance changes to evaluate the anti-reflective crack performance.
It realizes the anti-reflection crack performance evaluation of asphalt mixture under simulated actual pavement conditions under low cost and simple operation, and can objectively evaluate the suppression ability of asphalt mixture to reflective cracks, reduces the test cost, and is suitable for road surfaces at home and abroad. Material selection and mix optimization design.
Smart Images

Figure CN117871283B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an anti-reflective crack performance test of an asphalt mixture, and in particular to an indoor test method for testing the anti-reflective crack performance of an asphalt mixture, and belongs to the field of road engineering. Background Art
[0002] Semi-rigid bases represented by cement-stabilized crushed stone are widely used in the design and construction of high-grade highway asphalt pavements in my country due to their high bearing capacity and good integrity. In the application, a combination of thicker semi-rigid base and thinner asphalt concrete surface layer is generally used. However, there is often a large gap between the performance of semi-rigid base asphalt pavements and the design goals, and the service life is far from the design requirements. The main reason is that the semi-rigid base material has shrinkage characteristics and is prone to dry shrinkage and temperature shrinkage, resulting in early cracking; under the combined effects of the environment and load, the early cracks in the semi-rigid base will gradually extend upward, causing cracks in the asphalt pavement surface layer, that is, the occurrence of reflective crack disease.
[0003] In seasonally frozen areas with large temperature differences between day and night, severe winters, and frequent freeze-thaw cycles, the damage to semi-rigid base asphalt pavements is more significant, seriously affecting the pavement service performance and significantly increasing the subsequent maintenance costs. Therefore, accurately evaluating the anti-reflective cracking performance of asphalt mixtures is the basis for the prevention and control of reflective cracking diseases.
[0004] According to the generation and expansion mechanism of cracks, reflective cracks are mainly divided into two types: temperature type and load type. Indoor tests for evaluating the anti-reflective crack performance of asphalt mixtures also mainly include two categories: the first category is temperature-type reflective crack tests such as direct tensile test, bending fatigue test, indirect tensile test, semicircular bending test, impact toughness test and Overlay tester; the second category is load-type reflective crack tests such as three-point bending test, MTS fatigue loading test and improved rutting test.
[0005] However, in the above test methods, the single mechanical loading mode is difficult to truly reflect the reflection crack derivation process of asphalt mixtures, and the loading instruments are expensive, the test cost is high, and some test methods are designed by themselves, which are complicated to operate, time-consuming and labor-intensive, and have certain limitations. More importantly, they cannot simultaneously simulate the generation and development of temperature and load coupling reflection cracks caused by traffic loads and temperature stresses. In addition, the current reflection crack test mainly uses visual inspection to manually judge the appearance of cracks, and then measures the cracks by manual methods. However, the visual inspection method is only suitable for judging cracks with a width of more than 0.5 mm, lacks quantitative analysis, and is easily affected by human subjectivity. Therefore, it is urgent to seek a simple, practical, and indoor test method for the anti-reflection crack performance of asphalt mixtures that simulates traffic loads and temperature stresses at the same time, which can be used for the selection of pavement materials and the optimization design of mixtures.
[0006] In summary, the existing indoor tests on the anti-reflective cracking performance of asphalt mixtures have the problems of high cost and inability to objectively evaluate the ability of asphalt mixtures to suppress reflective cracks under the simultaneous coupling of traffic loads and temperature stresses. Summary of the invention
[0007] The purpose of the present invention is to solve the problems of high cost of existing indoor tests on the anti-reflective cracking performance of asphalt mixtures and the inability to objectively evaluate the ability of asphalt mixtures to suppress reflective cracks under the simultaneous coupling of traffic loads and temperature stresses, and to provide an indoor test method for testing the anti-reflective cracking performance of asphalt mixtures.
[0008] The technical solution of the present invention is:
[0009] An indoor test method for testing the anti-reflective cracking performance of asphalt mixture, comprising the following steps:
[0010] Step 1: Make pavement structure composite specimens:
[0011] The combined test specimen includes an asphalt mixture test specimen and a cement concrete test block layer; the cement concrete test block layer includes two cement blocks of the same size and arranged horizontally in parallel; the two cement blocks are pasted to the bottom of the asphalt mixture test specimen by heating and melting the asphalt adhesive, and a gap is reserved between the two cement blocks; the strain gauge is pasted to the lower edge of the front of the asphalt mixture test specimen, and the strain gauge is located in the gap between the two cement blocks;
[0012] Step 2: Specimen health care:
[0013] Place the combined specimen in step 1 in an environmental chamber for curing at a test temperature of ±0.5°C for more than 4 hours;
[0014] Step 3: Assemble the test piece fixture:
[0015] The specimen fixture includes a force transmission component and a displacement component; the force transmission component includes a first connecting rod, a second connecting rod, a third connecting rod and a fourth connecting rod, the first connecting rod and the second connecting rod are arranged front and back relative to each other to form a left connecting rod assembly, the third connecting rod and the fourth connecting rod are arranged front and back relative to each other to form a right connecting rod assembly, the upper and lower parts of the left connecting rod assembly and the right connecting rod assembly are both provided with circular openings, and the upper parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected through a round rod; the displacement component includes two square grooves and a bottom plate, the two square grooves are arranged side by side, the lower parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected to the two square grooves respectively, and the bottom end surfaces of the two square grooves are slidably mounted on the bottom plate;
[0016] Step 4: Carry out loading test:
[0017] The loading test is a repeated loading test. After the loading mode and loading frequency are determined, the strain gauge is connected to the strain demodulator, the combined specimen in step 1 is installed in the assembly specimen fixture, and a vertical load is applied to the round rods on the left connecting rod assembly and the upper part of the right connecting rod assembly of the specimen fixture;
[0018] Step 5: Anti-reflective crack performance evaluation:
[0019] The change in strain gauge resistance can reflect the development of cracks at the bottom of the asphalt mixture surface layer, and record the loading times N1, N2 and N3 when cracks appear, when cracks expand rapidly and when the specimen is destroyed, respectively, which serve as the main indicator for evaluating the anti-reflective crack performance of the mixture.
[0020] Furthermore, the asphalt mixture specimen in step one is a plate specimen prepared by wheel rolling method, static pressure method and vibration compaction method, and the asphalt mixture specimen is obtained by cutting. The dimensions of the asphalt mixture specimen are: length: 250±50mm, width: 50±5mm, height: 100±20mm.
[0021] Furthermore, the length of the cement concrete test block layer in step one is 120±20 mm, the width is 50±5 mm, and the height is 50±10 mm. A gap of 0.5 to 20 mm in width is reserved between the two cement concrete test block layers to simulate actual semi-rigid base cracks.
[0022] Furthermore, the middle sections of the first connecting rod, the second connecting rod, the third connecting rod and the fourth connecting rod of the assembled specimen fixture in step three are hollow, and the first connecting rod, the second connecting rod, the third connecting rod and the fourth connecting rod have the same structure and are all retractable in the length direction; wherein, the first connecting rod includes an upper U-shaped rod, a knob and a lower U-shaped rod, the opening sides of the upper U-shaped rod and the lower U-shaped rod are arranged relative to each other and plugged in, and the plug-in parts of the upper U-shaped rod and the lower U-shaped rod are connected and fixed by a knob.
[0023] Furthermore, in step three, a sliding groove is processed on the bottom plate along its length direction.
[0024] Furthermore, strip-shaped protrusions are processed on the bottom end surfaces of the two square grooves in step three, and the strip-shaped protrusions are slidably matched with the sliding grooves.
[0025] Furthermore, the temperature range of the loading test in step 4 is 5-50° C., the loading frequency is 0.1-50 Hz, the loading mode is load control or displacement control, and the loading waveform is a partial sine wave or a half sine wave.
[0026] Furthermore, in step 4, the stress level or strain level of the vertical load applied to the round rods on the upper parts of the left connecting rod assembly and the right connecting rod assembly of the specimen fixture ranges from 0.05 to 0.9.
[0027] Furthermore, the constraint angle between the upper part of the left connecting rod assembly and the right connecting rod assembly and the bottom of the two cement blocks is δ. When the loading mode is load control, the tension on the bottom of the two cement blocks is F = P × sinδ × cosδ, where P represents the vertical load applied to the round rod on the upper part of the left connecting rod assembly and the right connecting rod assembly of the specimen fixture, and the bending moment on the bottom is W = P × L × (sinδ) 2 , L represents the length of asphalt mixture specimen.
[0028] Preferably, the constraint angle δ is 30-45° or 45-60°.
[0029] Compared with the prior art, the present invention has the following effects:
[0030] 1. The test method for testing the anti-reflective cracking performance of asphalt mixture provided by the present invention is to prepare asphalt mixture plate specimens by adopting wheel rolling method, static pressure method and vibration compaction method, and put the prepared combined specimens into the specimen fixture, and conduct the test according to different test parameters on the specimen fixture. Through the flexible adjustment of the test parameters, it can well simulate the stress state of the surface asphalt mixture of the actual road surface during service when the semi-rigid base cracks and is subjected to bending (caused by traffic load) and tension (caused by temperature stress) at the same time, and the specimen assembly is convenient and the test operation is simple, and the anti-reflective cracking performance of the asphalt mixture can be objectively evaluated quickly and at low cost. In addition, it does not require independent research and development equipment, which effectively reduces the cost of indoor testing. Its standardized and standardized test process and test indicators make it widely used at home and abroad, and it has strong promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the overall structure of the combined test piece of the present invention; Figure 2 It is the overall structural diagram of the specimen fixture; Figure 3 yes Figure 2 Medium load transfer analysis diagram; Figure 4 It is a structural diagram of the connecting rod; Figure 5 It is a structural diagram of a square slot. DETAILED DESCRIPTION
[0032] Specific implementation method 1: Combination Figures 1 to 5 To illustrate this embodiment, the embodiment includes the following steps:
[0033] Step 1: Make pavement structure composite specimens:
[0034] The combined test specimen includes an asphalt mixture test specimen A and a cement concrete test block layer B; the cement concrete test block layer B includes two cement blocks B-1 arranged horizontally and in parallel and having the same size and two strain gauges B-2; the two cement blocks B-1 are pasted on the bottom of the asphalt mixture test specimen A by heating and melting the asphalt adhesive, and a gap is reserved between the two cement blocks B-1; the strain gauge B-2 is pasted on the lower edge of the front of the asphalt mixture test specimen A, and the strain gauge B-2 is located in the gap between the two cement blocks B-1;
[0035] Step 2: Specimen health care:
[0036] Place the combined specimen in step 1 in an environmental chamber for curing at a test temperature of ±0.5°C for more than 4 hours;
[0037] Step 3: Assemble the test piece fixture:
[0038] The specimen fixture includes a force transmission component C and a displacement component D; the force transmission component C includes a first connecting rod C-1, a second connecting rod C-2, a third connecting rod C-3 and a fourth connecting rod C-4, the first connecting rod C-1 and the second connecting rod C-2 are arranged front and back to form a left connecting rod assembly, the third connecting rod C-3 and the fourth connecting rod C-4 are arranged front and back to form a right connecting rod assembly, the upper and lower parts of the left connecting rod assembly and the right connecting rod assembly are both provided with circular openings C-5, and the upper parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected through a round rod; the displacement component D includes two square grooves D-1 and a bottom plate D-2, the two square grooves D-1 are arranged side by side, the lower parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected to the two square grooves D-1 respectively, and the bottom end surfaces of the two square grooves D-1 are slidably installed on the bottom plate D-2;
[0039] Step 4: Carry out loading test:
[0040] The loading test is a repeated loading test. After determining the loading mode and loading frequency, the strain gauge B-2 is connected to the strain demodulator, the combined specimen in step 1 is installed in the assembly specimen fixture, and a vertical load is applied to the round rods on the left and right connecting rod assemblies of the specimen fixture;
[0041] Step 5: Anti-reflective crack performance evaluation:
[0042] The change in resistance of strain gauge B-2 can reflect the development of cracks at the bottom of the asphalt mixture surface layer, and record the loading times N1, N2 and N3 when cracks appear, when cracks expand rapidly and when the specimen is destroyed, respectively, which serve as the main indicator for evaluating the anti-reflective crack performance of the mixture.
[0043] Specific implementation method 2: Combination Figure 1To illustrate this embodiment, the asphalt mixture specimen A in step 1 of this embodiment is a plate specimen prepared by wheel rolling method, static pressure method and vibration compaction method, and the asphalt mixture specimen is obtained by cutting. The dimensions of the asphalt mixture specimen A are: length: 250±50mm, width: 50±5mm, height: 100±20mm. Other components and connection relationships are the same as those in the specific embodiment 1.
[0044] Specific implementation method three: Combination Figure 1 This embodiment is described. The length of the cement concrete test block layer B in step 1 of this embodiment is 120±20 mm, the width is 50±5 mm, and the height is 50±10 mm. A gap of 0.5 to 20 mm is reserved between the two cement concrete test block layers B to simulate the cracks in the actual semi-rigid base. The other components and connection relationships are the same as those in the first or second embodiment.
[0045] Specific implementation method four: Combination Figure 2 and Figure 3 To explain this embodiment, the middle sections of the first connecting rod C-1, the second connecting rod C-2, the third connecting rod C-3 and the fourth connecting rod C-4 of the assembled specimen fixture in step three of this embodiment are hollow, and the first connecting rod C-1, the second connecting rod C-2, the third connecting rod C-3 and the fourth connecting rod C-4 have the same structure and are all retractable in the length direction; wherein, the first connecting rod C-1 includes an upper U-shaped rod, a knob and a lower U-shaped rod, the opening sides of the upper U-shaped rod and the lower U-shaped rod are arranged relatively and plugged in, and the plug-in parts of the upper U-shaped rod and the lower U-shaped rod are connected and fixed by a knob. This arrangement is made to reduce the influence of the deadweight of the connecting rod on the stress state of the specimen. Other components and connection relationships are the same as those of the specific embodiments one, two or three.
[0046] In addition, the first connecting rod C-1, the second connecting rod C-2, the third connecting rod C-3 and the fourth connecting rod C-4 in the present embodiment have the same structure, and there is a mechanism at the midpoint of the connecting rod, wherein the mechanism means that each connecting rod adopts an open-petal structure, such as the upper U-shaped rod and the lower U-shaped rod are two petals, and the open side rods of the upper U-shaped rod and the lower U-shaped rod are provided with a plurality of circular holes. When the upper U-shaped rod and the lower U-shaped rod are plugged in, when the circular holes of the upper U-shaped rod and the lower U-shaped rod coincide, an elastic knob is used for plug-in connection, and the length of the connecting rod is adjusted by different plug-in positions, thereby realizing flexible extension and retraction of the assembled specimen fixture; the four connecting rods form two parallel isosceles triangle truss structures on the front and back sides of the specimen, so that the structure is more stable during the test loading process.
[0047] Specific implementation method five: Combination Figure 2To explain this embodiment, in step 3 of this embodiment, a sliding groove is processed on the bottom plate D-2 along its length direction. This arrangement facilitates the square groove D-1 to slide smoothly on the bottom plate D-2. Other components and connection relationships are the same as those of the specific embodiments 1, 2, 3 or 4.
[0048] Specific implementation method six: Combination Figure 2 and Figure 5 To explain this embodiment, the bottom end surfaces of the two square grooves D-1 in step 3 of this embodiment are processed with strip protrusions, and the strip protrusions slide with the sliding grooves. This arrangement facilitates the two square grooves D-1 to slide along the length direction of the bottom plate D-2 during the test loading process. The other components and connection relationships are the same as those of the specific embodiments 1, 2, 3, 4 or 5.
[0049] The size of the stainless steel square groove used in the present invention can be freely adjusted and always remain the same as the size of the cement concrete test block, and there are sliding screws at the left / right lower corners of the front and rear surfaces of the square groove to fix the connecting rod. The angle between the connecting rod and the horizontal bottom plate can be adjusted by the position of the sliding screw.
[0050] Specific implementation method seven: Combination Figures 1 to 5 To illustrate this embodiment, the loading test temperature range in step 4 of this embodiment is 5 to 50°C, and the loading frequency is 0.1 to 50Hz. In seasonally frozen areas with large temperature differences between day and night, cold winters, and frequent freezing and thawing, thermal shrinkage cracks are prone to occur in semi-rigid base asphalt pavements. In view of the climatic characteristics of seasonally frozen areas, the above-mentioned test condition range is adopted. The loading mode is load control or displacement control, and the loading waveform is a partial sine wave or a half-sine wave. This setting is based on the classic periodic load model, considering that the car vibrates at a certain frequency and amplitude during driving on the road, and the overall state presents a periodic fluctuation, which is in line with the vibration characteristics of road traffic. Other components and connection relationships are the same as those of specific embodiments one, two, three, four, five or six.
[0051] Specific implementation method eight: Combination Figure 3 To illustrate this embodiment, in step 4 of this embodiment, the stress level or strain level of the vertical load applied to the round rods on the left connecting rod assembly and the upper part of the right connecting rod assembly of the specimen fixture is in the range of 0.05 to 0.9. With such a configuration, the stress level or strain level can be selected within the range of 0.05 to 0.9; a stepper motor is provided between the combined specimen and the specimen fixture to ensure that the fixture and the specimen are always in close contact in the strain-controlled loading mode. The other components and connection relationships are the same as those in the specific embodiments one, two, three, four, five or six.
[0052] Specific implementation method nine: Combination Figure 3To illustrate this embodiment, the constraint angle between the upper part of the left connecting rod assembly and the right connecting rod assembly and the bottom of the two cement blocks B-1 is δ, then the tension on the bottom of the two cement blocks B-1 is F = P × sinδ × cosδ, where P represents the vertical load applied to the round rod on the upper part of the left connecting rod assembly and the right connecting rod assembly of the specimen fixture, and the bending moment on the bottom is W = P × L × (sinδ) 2 , L represents the length of the asphalt mixture specimen. In this way, the asphalt mixture is subjected to bending and tension at the same time, which can simulate the generation and development of temperature and load coupling type reflective cracks caused by traffic load and temperature stress. The other components and connection relationships are the same as any one of the specific embodiments 1 to 8.
[0053] Specific implementation method ten: Combination Figure 3 To illustrate this embodiment, the constraint angle δ of this embodiment is 30-45° or 45-60°. With such a setting, for areas with severe cold or large temperature differences, the temperature load plays a dominant role, and δ should be in the range of 30-45°; for heavy-loaded highways, the traffic load plays a dominant role, and δ should be between 45-60°, which has a wide range of adaptability and is closer to the actual situation, ensuring the accuracy of the test. The other components and connection relationships are the same as any one of the specific embodiments one to nine.
[0054] Combination Figures 1 to 5 Describe the embodiments of the present invention:
[0055] (1) Prepare the combined specimens. The asphalt mixture rutting specimens are prepared by wheel rolling method. The asphalt mixture beam specimens are obtained by cutting. The dimensions are 250 mm in length, 50 mm in width and 100 mm in height. The asphalt used in the mixtures are 90# matrix asphalt, ordinary rubber asphalt, SX warm mix rubber asphalt and LN warm mix rubber asphalt, and the gradations are all ATB-25 gradation; the size of the cement concrete test block is 120 mm × 50 mm × 50 mm, and a 3 mm wide gap is reserved between the two test blocks; two cement blocks are glued to the bottom of the asphalt mixture specimen by heating and melting the rubber modified asphalt. After the assembly is completed, a 2 kg weight is placed to apply pressure and the specimen is left at room temperature for 12 hours; strain gauges are glued to the lower edges of the front and back sides of the asphalt mixture specimen;
[0056] (2) Assemble the fixture for the combined specimen, move the square grooves on the bottom plate of the fixture so that the gap between the square grooves is 3 mm; place the cement concrete test block of the combined specimen into the corresponding square groove, loosen the knob in the middle of the connecting rod, and then slide the screw at the lower left / right corner of the square groove to adjust the length of the connecting rod so that the horizontal angle δ of the connecting rod is 45°, and the round rod connecting the connecting rod is located at the midpoint of the top of the specimen;
[0057] (3) Anti-reflection crack test was carried out. At a test temperature of 15°C, a loading rate of 50 mm / min was used to carry out bending test of asphalt mixture beam specimens to test the destructive strength. The minimum temperature during the day and night in the seasonal freezing zone is relatively low, and the temperature difference between day and night is large. Therefore, three stress levels of 0.4, 0.5, and 0.6 were selected. Sine wave loading was used with a frequency of 10 Hz to carry out the test. The loading times N1, N2, and N3 of the three stages when cracks appeared, when cracks expanded rapidly, and when specimens were destroyed were recorded respectively. The results are shown in Table 1.
[0058] Table 1 Summary of loading times
[0059]
[0060] As shown in Table 1, with the increase of stress level, the number of loading times when cracks appeared, cracks expanded rapidly and specimens were destroyed in the four asphalt mixtures decreased significantly, indicating that the greater the load, the earlier the reflection cracks formed; under different stress levels, the number of loading times at each stage of the surface layers of different asphalt mixtures was the largest for LN warm mix asphalt mixture, the smallest for SX warm mix asphalt mixture, followed by rubber asphalt and matrix asphalt, which fully demonstrated that the anti-reflective crack performance of LN warm mix asphalt and rubber asphalt mixture was relatively excellent, the anti-reflective crack performance of SX warm mix asphalt mixture was the worst, and the ordinary matrix asphalt mixture was at an average level.
[0061] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture, characterized by: It includes the following steps: Step 1: Make pavement structure composite specimens: The combined specimen includes an asphalt mixture specimen (A) and a cement concrete specimen layer (B); the cement concrete specimen layer (B) includes two cement blocks (B-1) arranged horizontally and in parallel and having the same size and two strain gauges (B-2); Two cement blocks (B-1) are pasted to the bottom of the asphalt mixture specimen (A) by means of heated and melted asphalt adhesive, and a gap is reserved between the two cement blocks (B-1); a strain gauge (B-2) is pasted to the lower edge of the front of the asphalt mixture specimen (A), and the strain gauge (B-2) is located in the gap between the two cement blocks (B-1); Step 2: Specimen health care: Place the combined specimen in step 1 in an environmental chamber for curing at a test temperature of ±0.5°C for more than 4 hours; Step 3: Assemble the test piece fixture: The specimen fixture includes a force transmission component (C) and a displacement component (D); The force transmission component (C) comprises a first connecting rod (C-1), a second connecting rod (C-2), a third connecting rod (C-3) and a fourth connecting rod (C-4); the first connecting rod (C-1) and the second connecting rod (C-2) are arranged front and back to form a left connecting rod assembly; the third connecting rod (C-3) and the fourth connecting rod (C-4) are arranged front and back to form a right connecting rod assembly; the upper and lower parts of the left connecting rod assembly and the right connecting rod assembly are both provided with circular openings (C-5); the upper parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected via a round rod; The displacement member (D) comprises two square grooves (D-1) and a bottom plate (D-2), the two square grooves (D-1) are arranged side by side, the lower parts of the left connecting rod assembly and the right connecting rod assembly are rotatably connected to the two square grooves (D-1) respectively, and the bottom end surfaces of the two square grooves (D-1) are slidably mounted on the bottom plate (D-2); The middle sections of the first connecting rod (C-1), the second connecting rod (C-2), the third connecting rod (C-3) and the fourth connecting rod (C-4) of the assembled specimen fixture are hollow, and the first connecting rod (C-1), the second connecting rod (C-2), the third connecting rod (C-3) and the fourth connecting rod (C-4) have the same structure and are all retractable in the length direction; wherein the first connecting rod (C-1) comprises an upper U-shaped rod, a knob and a lower U-shaped rod, the opening sides of the upper U-shaped rod and the lower U-shaped rod are arranged oppositely and plugged, and the plug-in parts of the upper U-shaped rod and the lower U-shaped rod are connected and fixed by a knob; Step 4: Carry out loading test: The loading test is a repeated loading test. After the loading mode and loading frequency are determined, the strain gauge (B-2) is connected to the strain demodulator, the combined specimen in step 1 is installed in the specimen assembly fixture, and a vertical load is applied to the round rods on the left and right connecting rod assemblies of the specimen fixture; Step 5: Anti-reflective crack performance evaluation: The change in resistance of the strain gauge (B-2) can reflect the development of cracks at the bottom of the asphalt mixture surface layer, and record the loading times N1, N2 and N3 when cracks appear, when cracks expand rapidly and when the specimen is destroyed, respectively, which serve as the main indicators for evaluating the anti-reflective crack performance of the mixture.
2. The indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 1 is characterized in that: The asphalt mixture specimen (A) in step one is a plate specimen prepared by wheel rolling method, static pressure method and vibration compaction method. The asphalt mixture specimen is obtained by cutting. The dimensions of the asphalt mixture specimen (A) are: length: 250±50mm, width: 50±5mm, height: 100±20mm.
3. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 2, characterized in that: The length of the cement concrete test block layer (B) in step 1 is 120±20 mm, the width is 50±5 mm, and the height is 50±10 mm. A gap of 0.5 to 20 mm in width is reserved between the two cement concrete test block layers B to simulate the actual semi-rigid base cracks.
4. The indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 3 is characterized in that: The bottom plate (D-2) in step 3 is machined with sliding grooves along its length direction.
5. The indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 4 is characterized in that: The bottom end surfaces of the two square grooves (D-1) in step three are processed with strip-shaped protrusions, and the strip-shaped protrusions are slidably matched with the sliding grooves.
6. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 5, characterized in that: The temperature range of the loading test in step 4 is 5-40° C., the loading frequency is 0.1-50 Hz, the loading mode is load control or displacement control, and the loading waveform is a partial sine wave or a half sine wave.
7. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 6, characterized in that: In step 4, the stress level or strain level of the vertical load applied to the round rods on the upper part of the left connecting rod assembly and the right connecting rod assembly of the specimen fixture ranges from 0.05 to 0.
9.
8. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 7, characterized in that: The constraint angle between the upper part of the left connecting rod assembly and the right connecting rod assembly and the bottom of the two cement blocks (B-1) is δ. When the loading mode is load control, the tension on the bottom of the two cement blocks (B-1) is F = P × sinδ × cosδ, where P represents the vertical load applied to the round rod on the upper part of the left connecting rod assembly and the right connecting rod assembly of the specimen fixture, and the bending moment on the bottom is W = P × L × (sinδ) 2 , L represents the length of asphalt mixture specimen.
9. An indoor test method for testing the anti-reflective cracking performance of asphalt mixture according to claim 8, characterized in that: The constraint angle δ is 30 to 45° or 45 to 60°.