A detection method for analyzing the group of PVC products
By pounding and rolling in the mixer to form PVC samples of different combinations, the precipitation of heat stabilizer in PVC products is detected by color difference comparison, and the problems of large and inaccurate detection of blind spots in the prior art are solved, and rapid , accurate precipitation judgment, suitable for a variety of PVC materials.
Patent Information
- Application Number
- CN202410049573.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-01-12
AI Technical Summary
The prior art is difficult to effectively detect the precipitation of heat stabilizers in PVC products, especially when the degree of precipitation is low or non-black dark color materials, resulting in large blind spots in the test and it is difficult to accurately judge the degree of precipitation.
Using a detection method analyzed by PVC product group, the samples to be tested, the control samples and blank samples are formed by pounding and rolling in the mixing machine, and the color-developing color material is used, PVC resin, plasticizer and The combination of stabilizers can determine the degree of precipitation through color difference comparison, shorten the detection time and improve accuracy.
This method can quickly and accurately judge the precipitation of stabilizer in PVC products, reduce test blind spots, know the precipitation in advance, improve the production process, reduce raw material and equipment losses, and is suitable for non-black or dark color PVC materials.
Abstract
Description
Technical Field
[0001] The present application relates to the field of component detection, and in particular to a method for detecting component analysis of PVC products. Background Art
[0002] PVC is the abbreviation of polyvinyl chloride, which is one of the commonly used raw materials for products such as pipes, containers, and films. PVC products generally add additives to improve performance. For example, PVC has poor heat resistance, so in order to reduce thermal decomposition, heat stabilizers need to be added. In addition, PVC usually adds plasticizers, fillers, and modifying additives.
[0003] Sometimes, there is poor compatibility between heat stabilizers and PVC resins or other auxiliary components, which causes free fatty acids, calcium, sodium, magnesium, aluminum and other components in the heat stabilizers to precipitate on the surface of PVC products to form powder, resulting in poor appearance, reduced heat resistance, poor product printing and other problems. Therefore, after the production of PVC products is completed, it is usually necessary to test the precipitation of heat stabilizer components in PVC products.
[0004] The current testing method is: cut the PVC product into samples of a certain size, place the sample in a 70℃ oven for 24 hours, and then take it out to observe whether the surface of the sample turns white. If it turns white, it means precipitation. However, this method is mainly for black or dark PVC products, and it can only be observed when the precipitation is more serious. It is difficult to judge the situation of low precipitation, resulting in a blind spot in the test. Summary of the invention
[0005] In order to reduce the test blind area and facilitate the judgment of precipitation situation, the present application provides a method for detecting precipitation of PVC product groups.
[0006] The present application provides a method for detecting the group analysis of PVC products using the following technical solution:
[0007] A method for detecting the composition of PVC products, comprising the following steps:
[0008] Preparation of the test sample: putting the PVC composition to be tested into a clean open mill, pounding, rolling, forming the test sample on the roller surface of the open mill and taking it out; the PVC composition to be tested comprises PVC resin, plasticizer, stabilizer to be tested and coloring material;
[0009] Prepare a control sample: put the control PVC composition into an open mill, pound and roll, form a control sample on the roller surface of the open mill and take it out; the control PVC composition comprises PVC resin, plasticizer and stabilizer to be tested;
[0010] Prepare a blank sample: put the blank PVC composition into a clean open mill, pound and roll, form a blank sample on the roller surface of the open mill and take it out; the blank PVC composition contains PVC resin, plasticizer and stabilizer to be tested; compare the color difference between the control sample and the blank sample, judge the precipitation degree according to the color difference, and complete the detection.
[0011] By adopting the above technical solution, the coloring colorant has a weak compatibility with PVC. When a component in the stabilizer to be tested is precipitated, the coloring colorant will be precipitated together with it. In addition, since the sample to be tested is closely attached to the roller of the mixing mill during the rolling process, after the sample to be tested is taken out, the precipitated coloring colorant will still adhere to the roller. When the control PVC composition is rolled, the coloring colorant attached to the roller will be re-absorbed, so that the obtained control sample contains the coloring colorant and develops color. Finally, the blank sample is used as the chromaticity benchmark, and the color difference between the control sample and the blank sample is finally compared, and the degree of precipitation of the coloring colorant of the PVC composition to be tested is determined, thereby judging the precipitation degree of the stabilizer to be tested.
[0012] Compared with the existing method of making PVC products first and then sampling and testing, not only the testing time is greatly shortened, but also the method advances the detection step of the precipitated component, so as to know in advance the precipitation situation of the stabilizer to be tested in the PVC system. Therefore, the composition of the PVC product can be improved or adjusted according to the test results, and then production can be carried out, reducing the loss of raw materials and equipment operation. In addition, the coloring colorant is easier to observe and detect by colorimetry than the stabilizer component to be tested. Therefore, even if the PVC material is not black or dark in color, it can be detected and judged. The chromaticity comparison of the coloring colorant also makes the range of precipitation degree more broad, and the test blind area is small, which is convenient for judging the precipitation situation.
[0013] Optionally, the mass ratio of the PVC resin, the plasticizer, the stabilizer to be tested and the coloring colorant in the PVC composition to be tested is 100:(35-45):(1-3):(0.1-0.25).
[0014] Optionally, the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the control PVC composition is equal to the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the PVC composition to be tested, and the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the blank PVC composition is equal to the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the PVC composition to be tested.
[0015] By adopting the above technical solution, the basic formulas of the three samples are kept consistent, reducing variables, thereby further improving the accuracy of the test results.
[0016] Optionally, the roller temperature of the mixing mill is set to 165-170°C.
[0017] By adopting the above technical solution, the temperature of the above rollers is conducive to the full melting of the PVC composition and reduces the occurrence of PVC decomposition.
[0018] Optionally, the tamping is completed within 2 to 3 minutes, so that the PVC composition material evenly wraps the surface of the roller of the mixing mill, and the rolling time is 4 to 7 minutes.
[0019] By adopting the above technical solution, the material of the PVC composition fully wraps the roller, and the rolling time is controlled so that the formed sheet is in full contact with the roller surface, so that the thickness of the final sheet is uniform and can meet the requirements of the coloring colorant being precipitated in the first sheet and adsorbed in the second sheet.
[0020] Optionally, during the rolling process, the sample is coated on the roller of the rolling mill in the form of a thin sheet, and before taking out the sample, the sample is rolled into a solid cylindrical shape.
[0021] By adopting the above technical solution, the sample in the form of a thin sheet can be evenly attached to the roller, so that the colorant in the sample to be tested enters the control sample. The sample is in the form of a solid cylinder, making the color presented by the sample more obvious and easy to compare.
[0022] Optionally, the plasticizer is selected from one or more of dioctyl phthalate, di(2-ethylhexyl) phthalate, diisononyl phthalate and dioctyl terephthalate.
[0023] By adopting the above technical solution, the plasticizer makes the sample in a better refining state, and the above plasticizer is stable in PVC and is not easy to precipitate, so it is not easy to cause interference.
[0024] Optionally, the color developing pigment is carbon black.
[0025] By adopting the above technical solution, carbon black has a strong coloring ability for PVC, and the color is easy to observe. At the same time, the precipitated components of the stabilizer can easily bring out the carbon black, so carbon black is suitable as a coloring pigment.
[0026] Optionally, the stabilizer to be tested is selected from one or more of a composite stabilizer of calcium stearate and zinc stearate, a composite stabilizer of barium stearate and zinc stearate, an organic tin heat stabilizer and a phosphate heat stabilizer.
[0027] By adopting the above technical solution, the detection method can detect this type of thermal stabilizer.
[0028] Optionally, the step of preparing a blank sample is provided before the step of preparing the sample to be tested, and before the step of preparing the sample to be tested, the roller of the mixing mill is cleaned;
[0029] Alternatively, the step of preparing a blank sample is arranged after the step of preparing a control sample, and before the step of preparing the blank sample, the roller of the mixing mill is cleaned.
[0030] By adopting the above technical solution, since a small amount of coloring material may remain on the surface of the roller, the roller is cleaned before preparing the test sample or blank sample, thereby improving the accuracy of the detection.
[0031] In summary, this application has the following beneficial effects:
[0032] 1. The compatibility of coloring pigments with PVC is relatively weak. When a component in the stabilizer to be tested is precipitated, the coloring pigment will be precipitated together with it. In addition, since the sample to be tested is close to the roller of the mixing mill during the rolling process, the precipitated coloring pigment will still adhere to the roller after the sample to be tested is taken out. When the control PVC composition is rolled, the coloring pigment attached to the roller will be re-absorbed, so that the control sample obtained contains the coloring pigment and develops color. Finally, the blank sample is used as the chromaticity benchmark, and the color difference between the control sample and the blank sample is finally compared. The degree of precipitation of the coloring pigment of the PVC composition to be tested can be judged, thereby judging the precipitation degree of the stabilizer to be tested.
[0033] 2. Compared with the existing method of making PVC products first and then sampling and testing, not only the testing time is greatly shortened, but also the method advances the detection step of the precipitated component, so as to know in advance the precipitation of the stabilizer to be tested in the PVC system. Therefore, the composition of the PVC products can be improved or adjusted according to the test results, and then production can be carried out to reduce the loss of raw materials and equipment operation. In addition, the coloring colorant is easier to observe and detect by color than the stabilizer component to be tested. Therefore, even if the PVC material is not black or dark in color, it can be detected and judged. The chromaticity comparison of the coloring colorant also makes the range of precipitation degree more broad, and the test blind area is small, which is convenient for judging the precipitation situation. DETAILED DESCRIPTION
[0034] The present application is further described in detail below.
[0035] Example 1
[0036] A method for detecting the composition of PVC products, comprising the following steps:
[0037] The tested PVC composition, the control PVC composition and the blank PVC composition were prepared.
[0038] The PVC composition to be tested is composed of PVC resin, plasticizer, stabilizer to be tested and color-developing colorant, the mass ratio of PVC resin, plasticizer, stabilizer to be tested and color-developing colorant is 100:35:1:0.1, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate with a known large degree of precipitation; the color-developing colorant is specifically carbon black.
[0039] The control PVC composition consists of a PVC resin, a plasticizer and a stabilizer to be tested, the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested is 100:35:1, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate.
[0040] The blank PVC composition consists of PVC resin, plasticizer and stabilizer to be tested, the mass ratio of PVC resin, plasticizer and stabilizer to be tested is 100:35:1, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate.
[0041] The specific detection process is as follows:
[0042] S1. The PVC composition to be tested is mixed and put into an open mill. The roller temperature of the open mill is 165°C. The material of the PVC composition to be tested is plasticized under the friction shearing and extrusion of the two rollers, and the material is continuously cut and turned manually to complete the tamping. The tamping is completed within 2 minutes, so that the material of the PVC composition is evenly wrapped around the surface of the roller of the open mill. The rolling is continued for 7 minutes. During the rolling process, the sample is coated on the roller of the open mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a sample to be tested.
[0043] S2. After mixing, the control PVC composition is put into an open mill. The roller temperature of the open mill is 165°C. The material of the control PVC composition is plasticized, and the material is continuously cut and turned manually to complete the tamping. The tamping is completed within 2 minutes, so that the material of the PVC composition is evenly coated on the surface of the roller of the open mill. The rolling is continued for 7 minutes. During the rolling process, the sample is coated on the roller of the open mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a control sample.
[0044] S3. Clean the rollers of the mixing mill, then mix the blank PVC composition and put it into the mixing mill. The roller temperature of the mixing mill is 165°C. The blank PVC composition is plasticized and the material is manually cut and turned over to complete the tamping. The tamping is completed within 2 minutes, so that the PVC composition material is evenly coated on the surface of the rollers of the mixing mill. The rolling is continued for 7 minutes. During the rolling process, the sample is coated on the rollers of the mixing mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a blank sample.
[0045] S4. Use a gray card to compare the color difference between the control sample and the blank sample, determine the degree of precipitation based on the color difference, and complete the test.
[0046] Example 2
[0047] A method for detecting the composition of PVC products, comprising the following steps:
[0048] The tested PVC composition, the control PVC composition and the blank PVC composition were prepared.
[0049] The PVC composition to be tested is composed of PVC resin, plasticizer, stabilizer to be tested and color-developing colorant, the mass ratio of PVC resin, plasticizer, stabilizer to be tested and color-developing colorant is 100:45:3:0.25, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate with a known large degree of precipitation; the color-developing colorant is specifically carbon black.
[0050] The control PVC composition consists of a PVC resin, a plasticizer and a stabilizer to be tested, the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested is 100:45:3, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate.
[0051] The blank PVC composition consists of PVC resin, plasticizer and stabilizer to be tested, the mass ratio of PVC resin, plasticizer and stabilizer to be tested is 100:45:3, the plasticizer is specifically dioctyl phthalate; the stabilizer to be tested is specifically a composite stabilizer of calcium stearate and zinc stearate.
[0052] The specific detection process is as follows:
[0053] S1. The PVC composition to be tested is mixed and put into an open mill. The roller temperature of the open mill is 170°C. The material of the PVC composition to be tested is plasticized under the friction shearing and extrusion of the two rollers, and the material is continuously cut and turned manually to complete the tamping. The tamping is completed within 3 minutes, so that the material of the PVC composition is evenly wrapped around the surface of the roller of the open mill. The rolling is continued for 4 minutes. During the rolling process, the sample is coated on the roller of the open mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a sample to be tested.
[0054] S2. After mixing, the control PVC composition is put into an open mill. The roller temperature of the open mill is 170°C. The material of the control PVC composition is plasticized, and the material is continuously cut and turned manually to complete the tamping. The tamping is completed within 3 minutes, so that the material of the PVC composition is evenly coated on the surface of the roller of the open mill. The rolling is continued for 4 minutes. During the rolling process, the sample is coated on the roller of the open mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a control sample.
[0055] S3. Clean the rollers of the mixing mill, then mix the blank PVC composition and put it into the mixing mill. The roller temperature of the mixing mill is 170°C. The blank PVC composition is plasticized and the material is continuously cut and turned manually to complete the tamping. The tamping is completed within 3 minutes, so that the PVC composition material is evenly coated on the surface of the rollers of the mixing mill. Continue rolling for 4 minutes. During the rolling process, the sample is coated on the rollers of the mixing mill in the form of a thin sheet. Before taking out the sample, the sample is curled into a solid cylindrical shape to obtain a blank sample.
[0056] S4. Use a gray card to compare the color difference between the control sample and the blank sample, determine the degree of precipitation based on the color difference, and complete the test.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is that the stabilizer to be tested in the PVC composition to be tested is a composite stabilizer of calcium stearate and zinc stearate with a known low precipitation degree.
[0059] Comparative Example 1
[0060] A detection method for analyzing the group of PVC products:
[0061] The difference between this comparative example and Example 1 is that the PVC composition to be tested does not contain a coloring colorant.
[0062] Blank example 1
[0063] A comparative PVC composition was prepared, wherein the comparative PVC composition consisted of a PVC resin, a plasticizer and a stabilizer to be tested, and the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested was 100:45:3; the stabilizer to be tested was a composite stabilizer of calcium stearate and zinc stearate with a known large precipitation degree.
[0064] The comparative PVC composition was mixed and cast and extruded, and the screw temperature of the casting machine was 125° C. to obtain a light-colored PVC film.
[0065] The PVC film uses the existing detection method to detect the precipitation of stabilizers, as follows:
[0066] Cut the PVC film into samples with a length of 15 cm and a width of 5 cm. Place the samples in an oven at 70°C and bake for 24 hours. Then take them out and observe whether the surface of the samples turns white.
[0067] Blank example 2
[0068] A comparative PVC composition was prepared, wherein the comparative PVC composition consisted of a PVC resin, a plasticizer, a stabilizer to be tested and a dark colorant, the mass ratio of the PVC resin, the plasticizer, the stabilizer to be tested and the dark colorant being 100:45:3:0.5; the stabilizer to be tested was a composite stabilizer of calcium stearate and zinc stearate with a known large precipitation degree; and the dark colorant was specifically carbon black.
[0069] The comparative PVC composition was mixed and cast and extruded, and the screw temperature of the casting machine was 125° C. to obtain a dark PVC film.
[0070] The PVC film uses the existing detection method to detect the precipitation of stabilizers, as follows:
[0071] Cut the PVC film into samples with a length of 15 cm and a width of 5 cm. Place the samples in an oven at 70°C and bake for 24 hours. Then take them out and observe whether the surface of the samples turns white.
[0072] Blank example 3
[0073] A comparative PVC composition was prepared, wherein the comparative PVC composition consisted of a PVC resin, a plasticizer, a stabilizer to be tested and a dark colorant, the mass ratio of the PVC resin, the plasticizer, the stabilizer to be tested and the dark colorant being 100:45:3:0.5; the stabilizer to be tested was a composite stabilizer of calcium stearate and zinc stearate with a known low degree of precipitation; and the dark colorant was specifically carbon black.
[0074] The comparative PVC composition was mixed and cast and extruded, and the screw temperature of the casting machine was 125° C. to obtain a dark PVC film.
[0075] The PVC film uses the existing detection method to detect the precipitation of stabilizers, as follows:
[0076] Cut the PVC film into samples with a length of 15 cm and a width of 5 cm. Place the samples in an oven at 70°C and bake for 24 hours. Then take them out and observe whether the surface of the samples turns white.
[0077] Test results
[0078] The color difference between the control sample and the blank sample in the above Examples 1-3 and Comparative Example 1 was recorded, as shown in Table 1.
[0079] The observation results of the sample surfaces of Blank Examples 1-3 are recorded, as shown in Table 2.
[0080] Table 1
[0081] Color difference level Example 1 Level 3-4 Example 2 Level 3-4 Example 3 Level 4-5 Comparative Example 1 Level 5
[0082] Table 2
[0083] Observations Blank example 1 No whitening Blank example 2 There is obvious whitening phenomenon Blank example 3 Slight whitening
[0084] Combining Examples 1-3 with Blank Examples 1-3, it can be seen that the traditional detection method cannot determine whether the stabilizer of the light-colored PVC sample is precipitated, while the detection method of the present application can detect and determine the degree of precipitation of the PVC sample with the same formula, and the detection result is consistent with the actual situation. The degree of precipitation of the stabilizer can be clearly and intuitively reflected by the color difference level. Therefore, the test blind area is small, which is convenient for judging the precipitation situation, and the detection step is placed in front of the production step, which is efficient and cost-saving.
[0085] Combining Example 1 with Comparative Example 1, it can be seen that the stabilizer to be tested in the PVC composition to be tested is brought out by the coloring colorant, and the precipitation of the stabilizer to be tested itself does not develop color, so the accuracy is high.
[0086] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for detecting the composition of PVC products, characterized in that: The following steps are involved: Preparation of the test sample: putting the PVC composition to be tested into a clean open mill, pounding and rolling, forming the test sample on the roller surface of the open mill and taking it out; the PVC composition to be tested comprises PVC resin, plasticizer, stabilizer to be tested and coloring material; Preparing a control sample: putting a control PVC composition into the open mill of the above step of preparing the sample to be tested, pounding, rolling, forming a control sample on the roller surface of the open mill and taking it out; the control PVC composition comprises a PVC resin, a plasticizer and a stabilizer to be tested; since the coloring colorant precipitated in the step of preparing the sample to be tested will adhere to the roller, the control PVC composition will absorb the coloring colorant adhered to the roller during the open milling; Prepare a blank sample: put a blank PVC composition into a clean open mill, pound and roll, form a blank sample on the roller surface of the open mill and take it out; the blank PVC composition comprises a PVC resin, a plasticizer and a stabilizer to be tested; Comparing the color difference between the control sample and the blank sample, judging the degree of precipitation according to the color difference, and completing the detection; The mass ratio of the PVC resin, the plasticizer, the stabilizer to be tested and the coloring material in the PVC composition to be tested is 100:(35-45):(1-3):(0.1-0.25).
2. The method for detecting the composition of PVC products according to claim 1, characterized in that: The mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the control PVC composition is equal to the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the PVC composition to be tested, and the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the blank PVC composition is equal to the mass ratio of the PVC resin, the plasticizer and the stabilizer to be tested in the PVC composition to be tested.
3. The method for detecting the composition of PVC products according to claim 1, characterized in that: The roller temperature of the mixing mill is set at 165-170°C.
4. The method for detecting the composition of PVC products according to claim 1, characterized in that: The tamping is completed within 2 to 3 minutes, so that the PVC composition material evenly wraps the surface of the roller of the mixing mill, and the rolling time is 4 to 7 minutes.
5. The method for detecting the composition of PVC products according to claim 1, characterized in that: During the rolling process, the sample is wrapped around the roller of the rolling mill in the form of a thin sheet. Before taking out the sample, the sample is rolled into a solid cylindrical shape.
6. The method for detecting the composition of PVC products according to claim 1, characterized in that: The plasticizer is selected from one or more of dioctyl phthalate, di(2-ethylhexyl) phthalate, diisononyl phthalate and dioctyl terephthalate.
7. The method for detecting the composition of PVC products according to claim 1, characterized in that: The color developing pigment is carbon black.
8. The method for detecting the composition of PVC products according to claim 1, characterized in that: The stabilizer to be tested is selected from one or more of a composite stabilizer of calcium stearate and zinc stearate, a composite stabilizer of barium stearate and zinc stearate, an organic tin heat stabilizer and a phosphate heat stabilizer.
9. The method for detecting the composition of PVC products according to claim 1, characterized in that: The step of preparing a blank sample is arranged before the step of preparing the sample to be tested, and before the step of preparing the sample to be tested, the roller of the mixing mill is cleaned; Alternatively, the step of preparing a blank sample is arranged after the step of preparing a control sample, and before the step of preparing the blank sample, the roller of the mixing mill is cleaned.