A preparation method of temperature-responsive red phosphorescent material and the obtained product and application

Through the combination of large conjugated structure CDs and PMMA, a temperature-responsive red phosphorescent material is synthesized using a microwave heating method, which solves the problem of poor performance of stimulus-responsive phosphorescent materials in the existing technology and achieves red phosphorescence with high color saturation and contrast. The material is suitable for the field of information security and is simple to prepare and low cost.

CN117887463BActive Publication Date: 2024-10-29QUFU NORMAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410024092.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2024-10-29
Estimated Expiration
2044-01-08

AI Technical Summary

Technical Problem

Existing stimulus-responsive phosphorescent materials have problems such as strict selection of host materials, complex synthesis processes, and poor phosphorescent properties, which hinder their widespread application in the field of information security.

Method used

Using the hydrogen bonding behavior of CDs with a large conjugated structure and polymethylmethacrylate (PMMA) under different temperature conditions, a temperature-responsive red phosphorescent material was synthesized through a microwave-assisted heating method, and a rigid PMMA matrix was used to limit the non-radiative transition and regulate triplet energy gap, enabling significant phosphorescent color contrast from blue to red.

Benefits of technology

The prepared red phosphorescent material has high color saturation and contrast and is suitable for information security applications. The preparation method is simple, the raw materials are easily available, the cost is low, and it has broad application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117887463B_ABST
    Figure CN117887463B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite material preparation, and specifically relates to a method for preparing a temperature-responsive red phosphorescent material, and the resulting product and application. The present invention adopts a microwave-assisted heating method, uses pyrene as a carbon source, citric acid and biuret as reference materials, synthesizes two CDs, and embeds them into a PMMA matrix to obtain a red phosphorescent material that responds to temperature and has a significant color contrast. The present invention determines that a large conjugated structure and a high degree of graphitization effectively regulate the triplet state, resulting in a smaller singlet-triplet energy gap of the material. On the other hand, PMMA generates a large amount of hydroxyl groups during high-temperature pyrolysis, which in turn causes the amino and carboxyl groups on the surfaces of the two CDs to reorganize or break hydrogen bonds. Finally, temperature-responsive phosphorescence is generated. In addition, the rigid PMMA matrix hinders the non-radiative transition process, causing the phosphorescent material to emit blue fluorescence under ultraviolet irradiation and emit red phosphorescence when the irradiation stops.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and specifically relates to a preparation method of a temperature-responsive red phosphorescent material and the resulting product and application. Background Art

[0002] With the continuous improvement of information security standards, the application of information security in different environments has received widespread attention. At the same time, phosphorescent materials have the advantages of long luminescence time and good visual contrast, and have great application potential in the field of information security. In this context, various stimulus-responsive phosphorescent materials, such as humidity-responsive, ultraviolet-responsive, temperature-responsive, mechanical pressure-responsive and multi-stimulus-responsive phosphorescent materials have been explored. However, the host materials of stimulus-responsive phosphorescence have problems such as strict selection, complex synthesis process and poor phosphorescence performance, which seriously hinder the development of stimulus-responsive phosphorescence. Therefore, finding a high-performance stimulus-responsive phosphorescent material prepared from a single emission source has become a key development challenge.

[0003] Carbon-based nanoluminescent materials (carbon dots) are a new type of luminescent materials developed in recent years. They have the advantages of simple preparation and purification process, stable photophysical and chemical properties, adjustable emission characteristics, easy functional modification, good water solubility and biocompatibility, and have shown great application prospects in many fields such as chemical / biological sensing, bioimaging, medical diagnosis and treatment, photocatalysis and optoelectronic devices. However, in recent years, researchers have mainly focused on the regulation and preparation of the fluorescence properties of this type of material, the exploration of the luminescence mechanism and potential applications, and the research on its long-life luminescence performance is still relatively limited. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for preparing a temperature-responsive red phosphorescent material.

[0005] The present invention also provides a temperature-responsive red phosphorescent material prepared by the above preparation method.

[0006] Another object of the present invention is to provide an application of the temperature-responsive red phosphorescent material.

[0007] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:

[0008] The present invention provides a method for preparing a temperature-responsive red phosphorescent material, comprising the following steps:

[0009] (1) Pyrene, control material and AlCl 3 -6H 2O and then uniformly grind to obtain a solid mixture, and then subject the solid mixture to microwave treatment until the reaction is complete, cool to room temperature, and obtain control material @CDs powder, which is washed and purified with deionized water for later use;

[0010] (2) dissolving PMMA in DMF solution and allowing to stand to obtain a PMMA solution;

[0011] (3) Add the control material @CDs to the PMMA solution, ultrasonicate it until it is completely dissolved, drop-coat the mixed solution, and then cool and solidify it to obtain a sample film. The sample film is then dried to obtain the product.

[0012] Furthermore, in step (1), the pyrene, the reference material and AlCl 3 -6H 2 The mass ratio of O is 1.36:18-34:5.7.

[0013] Furthermore, in step (1), the control material is biuret (Bi) or citric acid (CA).

[0014] Furthermore, in step (1), the microwave treatment is firstly carried out at a power of 280-290 W for 30 min, and then at a power of 350-360 W for 20-30 min.

[0015] Furthermore, in step (2), the concentration of the PMMA solution is 0.2 g / mL.

[0016] Furthermore, in step (3), the ratio of the control material @CDs to PMMA is 1 mg:1 g.

[0017] Furthermore, the drying treatment is carried out at 70° C. for 60 minutes.

[0018] The present invention also provides a temperature-responsive red phosphorescent material prepared by the above preparation method.

[0019] The present invention also provides an application of the temperature-responsive red phosphorescent material in the field of information encryption and anti-counterfeiting.

[0020] The present invention provides a simple strategy to prepare high-performance temperature-induced red phosphorescent materials by utilizing the hydrogen bonding behavior of large conjugated CDs and polymethyl methacrylate (PMMA) under different temperature conditions. In this combination, the combination of rigid structure effectively restricts the non-radiative transition of the material, reduces energy loss, and achieves a clear phosphorescent color contrast (blue to red).

[0021] The present invention adopts microwave-assisted heating method, uses pyrene as carbon source, citric acid and biuret as control materials, synthesizes two CDs in one step, and embeds them into PMMA matrix to obtain a red phosphorescent material that responds to temperature and has significant color contrast (from blue fluorescence to red phosphorescence). Through various tests and characterization methods, the present invention determines that the large conjugated structure and high degree of graphitization effectively regulate the triplet state, resulting in the singlet-triplet energy gap (ΔE ST ) becomes smaller. On the other hand, PMMA generates a large number of hydroxyl groups during high-temperature pyrolysis. This in turn leads to the recombination or breaking of hydrogen bonds between the amino and carboxyl groups on the surfaces of the two CDs. Ultimately, temperature-responsive phosphorescence is produced. In addition, the rigid PMMA matrix hinders the non-radiative transition process, causing the phosphorescent material to emit blue fluorescence under ultraviolet irradiation and red phosphorescence when the irradiation stops.

[0022] The beneficial effects of the present invention are:

[0023] (1) The red phosphorescent material prepared by the present invention has high color saturation and contrast, making it an ideal choice for information security applications and has broad application potential and market prospects;

[0024] (2) The preparation method provided by the present invention is simple and quick, and the raw materials are easily available and low in cost, and a phosphorescent material with obvious response behavior under temperature stimulation is prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 UV-visible absorption spectra of different control material@CDs, where (a) is Bi@CDs and (b) is CA@CDs;

[0026] Figure 2 Raman spectra of different reference material@CDs, where (a) is Bi@CDs and (b) is CA@CDs;

[0027] Figure 3 XRD patterns of different control material@CDs, where (a) is Bi@CDs and (b) is CA@CDs;

[0028] Figure 4 Fourier transform infrared spectra of different reference material@CDs, where (a) is Bi@CDs and (b) is CA@CDs;

[0029] Figure 5 (a, b) XPS spectra of Bi@CDs and CA@CDs. (ce) High-resolution XPS fitting results of C1s, O1s and N1s spectra of Bi@CDs. (f, g) High-resolution XPS fitting results of C1s and O1s spectra of CA@CDs.

[0030] Figure 6 (a, b) Solid-state fluorescence (FL) and RTP emission spectra of Bi@CDs-C-PMMA and CA@CDs-H-PMMA. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further explained and illustrated by means of specific embodiments below.

[0032] Unless otherwise specified, the raw materials used in the preparation process of the present invention are all commercially available.

[0033] Example 1

[0034] (1) Synthesis of Bi@CDs

[0035] 1.36 mg of pyrene, 18 mg of biuret (Bi) and 5.7 mg of aluminum chloride hexahydrate (AlCl 3 -6H 2 O) was evenly ground in an agate mortar. The solid mixture was then poured into a beaker and treated in a microwave oven at 288 W for 30 minutes and heated at 360 W for 20 minutes until the reaction was complete. The mixture was cooled to room temperature to obtain Bi@CDs powder, which was then washed and purified with deionized water.

[0036] (2) Preparation of PMMA matrix

[0037] 2 g of PMMA was dissolved in 10 ml of DMF solution and allowed to stand overnight to obtain a PMMA solution;

[0038] (3) Preparation and heating treatment of Bi@CDs-PMMA composites

[0039] 2 mg Bi@CDs was added to the PMMA solution and ultrasonicated until completely dissolved. The mixed solution was drop-coated on a glass slide, cooled and solidified to obtain the sample film Bi@CDs-PMMA, and then the sample film was dried (70°C, 60 minutes). The products obtained by heating and cooling to room temperature are called Bi@CDs-H-PMMA and Bi@CDs-C-PMMA (H-heated to 70°C, C-cooled to room temperature).

[0040] Example 2

[0041] (1) Synthesis of CA@CDs

[0042] 1.36 mg of pyrene, 34 mg of citric acid (CA) and 5.7 mg of aluminum chloride hexahydrate (AlCl 3 -6H 2O) was evenly ground in an agate mortar. The solid mixture was then poured into a beaker and treated in a microwave oven at 288 W for 30 minutes and heated at 360 W for 20 minutes until the reaction was complete. The mixture was cooled to room temperature to obtain CA@CDs powder, which was then washed and purified with deionized water.

[0043] (2) Preparation of PMMA matrix

[0044] 2 g of PMMA was dissolved in 10 ml of DMF solution and allowed to stand overnight to obtain a PMMA solution;

[0045] (3) Preparation and heating treatment of CA@CDs-PMMA composites

[0046] 2 mg CA@CDs was added to the PMMA solution and ultrasonicated until completely dissolved. The mixed solution was drop-coated on a glass slide, cooled and solidified to obtain the sample film CA@CDs-PMMA, and then the sample film was dried (70°C, 60 minutes). The products obtained by heating and cooling to room temperature are called CA@CDs-H-PMMA and CA@CDs-C-PMMA (H-heated to 70°C, C-cooled to room temperature).

[0047] Effect Example

[0048] The materials prepared in Example 1-2 were characterized in terms of performance, specifically:

[0049] 1. From the UV-visible absorption spectrum Figure 1 a It can be determined that Bi@CDs has peaks at 270 nm, 306 nm and 324 nm, representing the π-π* transition and n-π* transition caused by C=O / C=N functional groups, respectively. Figure 1 b It can be determined that CA@CDs has peaks at 332 nm and 268 nm, representing the n-π* transition caused by the C=O functional group and the π-π* transition caused by the C=C functional group, respectively. It is inferred that the phosphorescence behavior of the material prepared in the present invention is caused by the combination of the large conjugated structure and the surface functional groups.

[0050] 2. Raman spectroscopy ( Figure 2 a, b) show that the Raman spectra peaks of Bi@CDs and CA@CDs are similar, located at 1404 and 1625 cm -1 The intensity ratio of the D band to the G band of Bi@CDs and CA@CDs (I D / I G ) are 1.11 and 1.09 respectively, which indicates that there are certain structural defects in the two CDs.

[0051] 3. The present invention analyzes the elements and chemical compositions of Bi@CDs and CA@CDs by XRD. Figure 3 a, b show that the XRD spectra of both CDs have three peaks, and Bi@CDs and CA@CDs have a prominent peak at 23°, corresponding to the (002) crystal plane of carbon. A clear peak at 24° for Bi@CDs and CA@CDs indicates the presence of the (002) crystal plane in graphitic carbon. On the other hand, the narrow diffraction peaks of Bi@CDs and CA@CDs at around 28° also indicate that they have obvious graphite structural characteristics. This shows that both materials have good crystallinity and both exhibit a highly graphitized structure.

[0052] 4. Analyze the chemical bonds of Bi@CDs and CA@CDs using Fourier transform infrared spectroscopy (FTIR). Figure 4 As shown in a, Bi@CDs at 3412 cm -1 The absorption peaks at 1714 and 1497 cm are caused by the stretching vibration of the NH functional group. -1 The absorption peaks at 1609 and 831 cm are caused by the stretching vibration of the C=O functional group. -1 The absorption peaks at are the stretching vibrations caused by the C-N and C-H functional groups. Figure 4 b Characterization of the infrared absorption peaks of CA@CDs, such as 1714, 1637, and 1399 cm -1 The absorption peaks at 1181 and 837 cm-1 of CA@CDs are mostly caused by the stretching vibration of the C=O functional group. -1 The peaks at are due to the stretching vibrations of CO and CH functional groups. The Fourier transform infrared spectroscopy results show that Bi@CDs and CA@CDs are composed of sp 2 It consists of a conjugated carbon core and surface functional groups.

[0053] 5. The existence of elements and functional groups in Bi@CDs and CA@CDs was further confirmed by X-ray photoelectron spectroscopy (XPS). Figure 5 As shown in a, Bi@CDs is composed of C, O, and N elements. The C1s, O1s, and N1s peaks are at 281 eV, 529 eV, and 396 eV, respectively, and the atomic ratio is C:O:N=49:27:24. The C1s XSP spectrum of Bi@CDs has three peaks at 283.3 eV, 284.8 eV, and 288 eV, which belong to CC / CH, C=C, and C=O, respectively. Figure 5 c). The O1s XSP spectrum of Bi@CDs has a peak at 527.5 eV, which belongs to C=O ( Figure 5d). The N1s XSP spectrum of Bi@CDs has two peaks at 398.4 eV and 399.4 eV, belonging to NC and NH, respectively. Figure 5 e). On the other hand, the C1s and O1s peaks of CA@CDs are at 282 eV and 529 eV, respectively, and the atomic ratio is C:O=67:36 ( Figure 5 b). The C1s XSP spectrum of CA@CDs has three peaks at 280.7 eV, 282 eV and 284.9 eV, belonging to CC / C=C, CO and C=O respectively ( Figure 5 f). The O1s XSP spectrum of CA@CDs has two peaks at 528 eV and 529.2 eV, belonging to O=C and OC, respectively. The similarity between the FTIR and XPS data suggests that the material surface has a wide range of functional groups, which has a significant impact on its optical properties. In addition, these findings verify the necessary molecular basis for achieving phosphorescence at the structural level.

[0054] 6. Figure 6 The fluorescence emission of the two materials under 360 nm excitation and the phosphorescence emission when the excitation is turned off are shown. Both Bi@CDs-C-PMMA and CA@CDs-H-MMA have blue emission at 393 nm. After turning off the excitation, their phosphorescence emission peaks are located at 656 nm and 674 nm, resulting in a wavelength difference of about 260 nm, indicating that the materials have achieved phosphorescence emission from blue to red.

Claims

1. A method for preparing a temperature-responsive red phosphorescent material, characterized in that: The following steps are involved: (1) Pyrene, a reference material and AlCl3-6H2O are mixed and uniformly ground to obtain a solid mixture, and then the solid mixture is subjected to microwave treatment until the reaction is complete, cooled to room temperature, and a reference material@CDs powder is obtained, which is washed and purified with deionized water for later use; The control material is biuret or citric acid (2) dissolving PMMA in DMF solution and allowing to stand to obtain a PMMA solution; (3) Add the control material @CDs to the PMMA solution, ultrasonicate it until it is completely dissolved, drop-coat the mixed solution, and then cool and solidify it to obtain a sample film. The sample film is then dried to obtain the product.

2. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of pyrene, reference material and AlCl3-6H2O is 1.36:18-34:5.

7.

3. The preparation method according to claim 1 or 2, characterized in that: In step (1), the microwave treatment is firstly carried out at a power of 280-290 W for 30 min, and then at a power of 350-360 W for 20-30 min.

4. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the PMMA solution is 0.2 g / mL.

5. The preparation method according to claim 1, characterized in that: In step (3), the ratio of the control material @CDs to PMMA is 1 mg:1 g.

6. The preparation method according to claim 1 or 5, characterized in that: The drying process is carried out at 70° C. for 60 min.

7. A temperature-responsive red phosphorescent material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the temperature-responsive red phosphorescent material as claimed in claim 7 in the field of information encryption and anti-counterfeiting.

Citation Information

Patent Citations

  • Oil-solubility carbon quantum dots (OCDs), PMMA-coated OOCDs, and preparation method and application thereof

    CN106916587A

  • Preparation method of mechanofluorescent color-adjustable carbon dot

    CN110564414A