A method for preparing a diaphragm for electrolysis of alkaline water

Through the preparation of multi-layer structured membranes of polyphenylene sulfide and sulfonated polyether ether ketone, the problem of insufficient gas barrier properties and mechanical strength in the hydrogen production process of electrolytic alkali water is solved, and low-cost and efficient membrane preparation is achieved , suitable for large-scale industrial production.

CN117899676BActive Publication Date: 2024-11-12JIANGYIN HENNENG HYDROGEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410099854.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-12
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

In the existing process of electrolytic alkali water hydrogen production, the gas barrier and mechanical strength of the membrane are insufficient, and the preparation process cost is high, making it difficult to achieve large-scale industrial production.

Method used

Composite fibers using polyphenylene sulfide and sulfonated polyether ether ketone are melt-spinned and surface-treated to form barrier layers. Combined with nanotitanium dioxide and polyethyleneimine and other materials to form a multi-layered membrane, through a specific process flow Such as dispersion and slurrying, hot pressing, alkalizing treatment, etc., a diaphragm with high gas barrier properties and mechanical strength is prepared.

Benefits of technology

The high gas barrier and mechanical strength of the separator in the electrolytic alkali water hydrogen production process is achieved, the preparation process cost is reduced, and it is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004679860540000081
    Figure BDA0004679860540000081
Patent Text Reader

Abstract

The invention discloses a method for preparing a diaphragm for electrolyzing alkaline water, which comprises preparing a hydrophilic base film, and forming a barrier layer on the surface of the diaphragm after surface treatment, so as to obtain a diaphragm for electrolysis with a multilayer structure using the base film as a skeleton. The diaphragm has good gas barrier properties and high mechanical strength in the process of electrolyzing alkaline water to produce hydrogen, and the preparation process cost is low, and it is easy to be mass-produced industrially.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials and engineering technology, and in particular relates to a method for preparing a diaphragm for electrolyzing alkaline water. Background Art

[0002] In recent years, with the increasing prominence of global warming, energy shortages and price increases, people have begun to look for alternatives to traditional petrochemical energy. After decades of development, the renewable energy industry represented by wind energy, solar energy and hydrogen energy has made great progress, and its use price is rapidly approaching the price of traditional petrochemical energy. Among them, hydrogen, as an energy carrier, can not only meet global energy needs, but also reduce CO2 emissions, and play an important role in the future development of the energy industry. Among the current mainstream hydrogen production methods, fossil energy hydrogen production and industrial by-product hydrogen still have carbon emissions, and green hydrogen is the mainstream in the future. Among them, the use of renewable energy (wind energy, photovoltaics, etc.) to produce green hydrogen is the future development direction. Large-scale water electrolysis hydrogen production technology is the key to the efficient use of green hydrogen.

[0003] Hydrogen production by water electrolysis has the advantages of mature technology, high product purity, and environmental friendliness. It is an important technical means for modern large-scale production of hydrogen. Alkaline water electrolyzer is the main equipment for water electrolysis hydrogen production. The electrolyzer is divided into an anode chamber and a cathode chamber by a diaphragm, and an anode and a cathode are set separately. KOH or NaOH solution is used as the electrolyte in the electrolyzer to obtain oxygen at the anode and hydrogen at the cathode. The diaphragm set between the anode chamber and the cathode chamber is used to prevent the mixing of hydrogen and oxygen. In the alkaline water electrolysis hydrogen production equipment, the electrolyzer is the core component. The diaphragm has two main functions. One is to act as an insulating layer to separate the anode and cathode to avoid short circuit between the two poles; the other is to be hydrophilic and gas-repellent, which can allow the alkaline solution to pass through the diaphragm while separating hydrogen and oxygen to avoid hydrogen and oxygen from mixing. Summary of the invention

[0004] The invention discloses a method for preparing a diaphragm for electrolyzing alkaline water, which comprises preparing a hydrophilic base film, and forming a barrier layer on the surface of the diaphragm after surface treatment, so as to obtain a diaphragm for electrolysis with a multilayer structure using the base film as a skeleton. The diaphragm has good gas barrier properties and high mechanical strength in the process of electrolyzing alkaline water to produce hydrogen, and the preparation process cost is low, and it is easy to be mass-produced industrially.

[0005] The present invention provides a method for preparing a diaphragm for electrolyzing alkaline water, comprising:

[0006] 1) mixing polyphenylene sulfide and sulfonated polyetheretherketone in a mass ratio of 100:15-20, and performing melt spinning to obtain composite fibers;

[0007] 2) putting the fibers from step 1) into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film;

[0008] 3) placing the diaphragm of step 2) in a sodium hydroxide solution and heating it; then washing it with deionized water until it is neutral; drying the base film and then performing plasma surface treatment in air;

[0009] 4) adding polysulfone, carboxymethyl cellulose, nano titanium dioxide, polyethyleneimine, and hexadecyltrimethylammonium bromide into NMP and stirring until completely dissolved to obtain a casting solution;

[0010] 5) The casting solution is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing sodium carbonate, glutaraldehyde and diethylene glycol at 48-52° C. for 15-20 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0011] Furthermore, in step 1), polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:15-20, melt-spun, and cut to obtain fibers with a fineness of 2-3 μm and a length of 20-30 mm, wherein the melt index of polyphenylene sulfide and sulfonated polyetheretherketone is 20-25 g / min.

[0012] Furthermore, in step 2), the pulping concentration is 3-5wt%, the papermaking concentration is 0.5-0.8%, the hot pressing pressure is 15-20Mpa, and the hot pressing temperature is 200-240°C.

[0013] Furthermore, in step 3), the concentration of the sodium hydroxide solution is 2-4 mol / L, the heating temperature is 80-100°C, and the temperature is maintained for 2-4 hours; the intensity of the plasma surface treatment is 150-200 KW·s / m 2 .

[0014] Furthermore, in step 4), 10-15 parts by mass of polysulfone, 1-2 parts by mass of carboxymethyl cellulose, 5-10 parts by mass of titanium dioxide, 2-4 parts by mass of polyethyleneimine, and 1-3 parts by mass of hexadecyltrimethylammonium bromide are added to 60-70 parts by mass of NMP.

[0015] Furthermore, in step 5), the aqueous solution contains 5-8 wt% sodium carbonate, 12-15 wt% glutaraldehyde and 10-20 wt% diethylene glycol.

[0016] A diaphragm for electrolyzing alkaline water, wherein the diaphragm is prepared by adopting the preparation method.

[0017] The invention discloses an application of a diaphragm for electrolyzing alkaline water, wherein the diaphragm is used for electrolyzing alkaline water to produce hydrogen.

[0018] The present invention has the following beneficial effects:

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] 1) The base film obtained by adding sulfonated polyetheretherketone to polyphenylene sulfide has better mechanical properties. Compared with polyetheretherketone, sulfonated polyetheretherketone with a sulfonation degree of 10% has relatively higher corrosion resistance;

[0021] 2) Since polyetheretherketone will become brittle under the action of ultraviolet rays, which will affect the life of the diaphragm, adding nano titanium dioxide to the casting solution can absorb ultraviolet rays and increase the service life of the diaphragm. At the same time, the ion conduction and hydrophilic effect of titanium dioxide can reduce the resistance of the diaphragm and improve the liquid retention performance;

[0022] 3) The base film is alkalized and surface ionized to improve the bonding between the base film and the barrier layer. At the same time, the characteristics of polyethyleneimine and glutaraldehyde that can be cross-linked into a network structure at around 50°C are used to

[0023] The components in the casting solution are firmly fixed on the surface of the base film;

[0024] 4) The diaphragm of the present invention has good gas barrier properties and high mechanical strength in the process of producing hydrogen by electrolysis of alkaline water, and the preparation process cost is low, and it is easy to be mass-produced industrially. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific embodiments. However, the protection scope of the present invention is not limited to the following embodiments, and any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.

[0026] Example 1

[0027] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:15, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0028] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0029] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 2 mol / L, heating at 100°C for 4 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 200 KW·s / m 2 ;

[0030] 4) adding 10 parts by mass of polysulfone, 1 part by mass of carboxymethyl cellulose, 5 parts by mass of titanium dioxide, 2 parts by mass of polyethyleneimine, and 1 part by mass of hexadecyltrimethylammonium bromide to 60 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0031] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 5wt% sodium carbonate, 12wt% glutaraldehyde and 10wt% diethylene glycol at 52°C for 15 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0032] Example 2

[0033] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:20, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0034] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0035] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 4 mol / L, heating at 80°C for 2 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 150 KW·s / m 2 ;

[0036] 4) adding 15 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 10 parts by mass of titanium dioxide, 4 parts by mass of polyethyleneimine, and 3 parts by mass of hexadecyltrimethylammonium bromide to 70 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0037] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 8wt% sodium carbonate, 15wt% glutaraldehyde and 20wt% diethylene glycol at 48°C for 20 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0038] Example 3

[0039] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:18, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0040] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0041] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 3 mol / L, heating at 90°C for 3 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 180 KW·s / m 2 ;

[0042] 4) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 8 parts by mass of titanium dioxide, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0043] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 50°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0044] Comparative Example 1

[0045] 1) melt spinning polyphenylene sulfide and cutting to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt index of the polyphenylene sulfide is 20 g / min;

[0046] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0047] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 3 mol / L, heating at 90°C for 3 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 180 KW·s / m 2 ;

[0048] 4) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0049] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 50°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0050] Comparative Example 2

[0051] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:18, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0052] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0053] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 3 mol / L, heating at 90°C for 3 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 180 KW·s / m 2 ;

[0054] 4) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0055] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 50°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0056] Comparative Example 3

[0057] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:18, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0058] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0059] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 3 mol / L, heating at 90°C for 3 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 180 KW·s / m 2 ;

[0060] 4) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 8 parts by mass of titanium dioxide, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0061] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 40°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0062] Comparative Example 4

[0063] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:18, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0064] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0065] 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 3 mol / L, heating at 90°C for 3 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 180 KW·s / m 2 ;

[0066] 4) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 8 parts by mass of titanium dioxide, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0067] 5) The casting liquid is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 60°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0068] Comparative Example 5

[0069] 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:18, melt-spinned, and cut to obtain fibers with a fineness of 3 μm and a length of 25 mm, wherein the melt indexes of polyphenylene sulfide and sulfonated polyetheretherketone are 20 g / min and 25 g / min, respectively;

[0070] 2) The fibers of step 1) are put into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; the pulping concentration is 4wt%, the papermaking concentration is 0.6%, the hot pressing pressure is 16Mpa, and the hot pressing temperature is 220°C;

[0071] 3) adding 12 parts by mass of polysulfone, 2 parts by mass of carboxymethyl cellulose, 8 parts by mass of titanium dioxide, 3 parts by mass of polyethyleneimine, and 2 parts by mass of hexadecyltrimethylammonium bromide to 65 parts by mass of NMP, and stirring for 0.5 h to obtain a casting solution;

[0072] 4) The casting solution is scraped onto the base film obtained in step 2), and then immersed in an aqueous solution containing 6wt% sodium carbonate, 12wt% glutaraldehyde and 15wt% diethylene glycol at 50°C for 16 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

[0073] Performance Testing

[0074] The porosity of the separators of the embodiments of the present invention and the comparative examples is 45±2%, the pore diameter is 5±0.2 μm, and the thickness is 400±5 μm.

[0075] Bubble point test method: Cut the diaphragm into small pieces, soak it with high-purity water, and put it into the bubble pressure membrane pore size analyzer (BSD-PB) for testing. Apply gas pressure on one side of the membrane. When a gas flow of 1 mL / min is detected on the other side of the membrane, the pressure is regarded as the bubble point of the diaphragm.

[0076] After being immersed in 40wt% KOH solution for 12h, the resistance was tested using an electrochemical workstation.

[0077] For breaking strength, refer to GB / T3923.1-2013.

[0078] The diaphragm was placed in a 30 wt % KOH solution and heated to 80° C. for 300 h, and the breaking strength loss rate was calculated: strength loss rate = breaking strength difference before and after heat treatment / breaking strength before heat treatment.

[0079] Table 1

[0080]

[0081] Results Data

[0082] The addition of sulfonated polyetheretherketone with a sulfonation degree of 10% makes the diaphragm have better mechanical properties;

[0083] The addition of titanium dioxide reduces the strength loss rate. At the same time, the ion conduction and hydrophilic effect of titanium dioxide can reduce the resistance of the diaphragm and improve the liquid retention performance.

[0084] The base membrane is alkalized and the surface is ionized to improve the bonding between the base membrane and the barrier layer and the mechanical properties of the diaphragm;

[0085] By utilizing the property that polyethyleneimine and glutaraldehyde can cross-link into a network structure at around 50°C, the components in the casting solution are firmly fixed on the surface of the base film, thereby improving the gas barrier properties of the separator.

[0086] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.

Claims

1. A method for preparing a diaphragm for electrolysis of alkaline water, It is characterized in that include: 1) polyphenylene sulfide and sulfonated polyetheretherketone with a sulfonation degree of 10% are mixed in a mass ratio of 100:15-20, melt-spinned, and cut to obtain fibers with a fineness of 2-3 μm and a length of 20-30 mm, wherein the melt index of polyphenylene sulfide and sulfonated polyetheretherketone is 20-25 g / min; 2) putting the fibers from step 1) into deionized water for dispersion, pulping, debonding, papermaking, and hot pressing to obtain a base film; 3) placing the diaphragm of step 2) in a sodium hydroxide solution with a concentration of 2-4 mol / L, heating at 80-100°C for 2-4 hours; then washing with deionized water until neutral; drying the base film, and then performing plasma surface treatment in air, the intensity of the plasma surface treatment being 150-200 KW·s / m 2 ; 4) adding 10-15 parts by mass of polysulfone, 1-2 parts by mass of carboxymethyl cellulose, 5-10 parts by mass of titanium dioxide, 2-4 parts by mass of polyethyleneimine, and 1-3 parts by mass of hexadecyltrimethylammonium bromide to 60-70 parts by mass of NMP, and stirring until completely dissolved to obtain a casting solution; 5) The casting solution is scraped onto the modified base film obtained in step 3), and then immersed in an aqueous solution containing 5-8wt% sodium carbonate, 12-15wt% glutaraldehyde and 10-20wt% diethylene glycol at 48-52° C. for 15-20 minutes. After being taken out, it is washed with deionized water and dried to obtain a diaphragm for electrolysis of alkaline water.

2. A method for preparing a diaphragm for electrolysis of alkaline water as claimed in claim 1, Features: In step 2), the pulping concentration is 3-5wt%, the papermaking concentration is 0.5-0.8%, the hot pressing pressure is 15-20Mpa, and the hot pressing temperature is 200-240°C.

3. A diaphragm for electrolysis of alkaline water, It is characterized in that The diaphragm is prepared by the preparation method according to any one of claims 1 to 2.

4. An application of the diaphragm according to claim 3, wherein the diaphragm is used for producing hydrogen by electrolyzing alkaline water.