A method for preparing spherical micro-nano silicon dioxide by using metal silicon powder deflagration method

By introducing metallic silicon powder into a high-temperature flame and deflagrating it, spherical micro-nano silica is produced, which solves the problems of high cost and safety hazards of high-temperature silicon melting and heated pure oxygen in the slurry method, and achieves more stable silica preparation. process and product.

CN117902583BActive Publication Date: 2024-10-25SHANDONG JINWEI NANO TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410104638.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2024-10-25
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

Among the existing spherical micro-nano silica manufacturing methods, the slurry method involves high-temperature silicon melting and heated pure oxygen, which has problems of high cost and potential safety hazards.

Method used

Spherical micro-nano silica is produced by using metal silicon powder that is introduced into a high-temperature flame by an inert gas protective cyclone and deflagrated. After the metal silicon powder is cut into appropriate particle sizes, it is evenly introduced into the high-temperature flame formed by combustible gas and oxygen for deflagration. Silica is produced.

Benefits of technology

The production cost is reduced, safety hazards are avoided, and the spherical silica obtained has a more stable structure and more complete melting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117902583B_ABST
    Figure CN117902583B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of nano silicon dioxide, and discloses a method for preparing spherical micro-nano silicon dioxide by using a metal silicon powder deflagration method. The present invention obtains metal silicon powder from a metal silicon block, and then uniformly introduces the metal silicon powder into a high-temperature flame formed by the combustion of a combustible gas and oxygen under the protection of an inert gas to deflagrate, reacts with oxygen to generate silicon dioxide, and is melted at a high temperature to prepare spherical micro-nano silicon dioxide. The present invention uses a method for preparing spherical micro-nano silicon dioxide by using a metal silicon powder deflagration method. By using an inert gas cyclone protective feeding, the problem of uneven feeding and insufficient deflagration caused by oxidation of the front surface of the silicon powder is solved, thereby improving production efficiency. Compared with other slurry production methods, it greatly reduces costs and improves safety and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano silicon dioxide, in particular to a method for preparing spherical micro-nano silicon dioxide by utilizing a metallic silicon powder deflagration method. Background Art

[0002] Micro-nano materials have special properties such as surface effect, small size, optical effect, quantum size effect, etc., which can effectively improve the mechanical and mechanical properties of molecular materials. Silicon dioxide is an inorganic compound widely used in glass, pottery, cement, glaze and other fields.

[0003] Micro-nano silica has the characteristics of small particle size and large specific surface area, and therefore has excellent reinforcement, thickening, matting, anti-adhesion and other properties. It is widely used in coatings, medicine, papermaking and other fields. Moreover, with the development of science and technology society, the demand for micro-nano silica is increasing.

[0004] Among them, spherical silicon dioxide is widely used in the fields of semiconductor packaging, substrates, etc., and one of the methods for manufacturing spherical silicon dioxide is to melt metal silicon powder at high temperature to make slurry, heat pure oxygen to 1000 degrees, and then introduce it into the reactor for deflagration to obtain spherical silicon dioxide. This method is not only costly, but also has great safety hazards in the production process. Therefore, how to reduce and avoid safety hazards in the preparation process of spherical silicon dioxide is one of the current research focuses. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing spherical micro-nano silicon dioxide by utilizing the metal silicon powder deflagration method. The present invention utilizes the method of introducing metal silicon powder into a high-temperature flame through an inert gas-protected cyclone to deflagrate to prepare spherical micro-nano silicon dioxide, which solves the problems of high cost and potential safety hazards when using a slurry method to melt silicon at high temperature and heat pure oxygen.

[0006] A method for preparing spherical micro-nano silicon dioxide by using a metal silicon powder deflagration method, the preparation method is as follows:

[0007] The metal silicon block is cut into metal silicon powder, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by combustible gas and oxygen through an inert gas for explosion to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0008] Preferably, in the step, the D50 particle size of the metal silicon powder obtained by cutting is 1-1.5 microns, the D10 particle size is 0.1-0.5 microns, and the particle size of the metal silicon powder is 1000 nanometers.

[0009] Preferably, in the steps, the inert gas is nitrogen, and the combustible gas is one or both of natural gas and acetylene.

[0010] Preferably, in the step, the feeding amount of the metallic silicon powder when introduced into the high-temperature flame is 350-380 kg / hour.

[0011] Preferably, in the step, the supply rate of the inert gas is set to 40-60 cubic meters per hour.

[0012] Preferably, in the steps, the oxygen supply rate is set to 650-720 cubic meters per hour.

[0013] Preferably, in the steps, the supply rate of the combustible gas is set to 350-400 cubic meters per hour.

[0014] Preferably, in the steps, the temperature of the high-temperature flame formed by the combustion of the combustible gas and oxygen during the deflagration process is 2000-2400 degrees.

[0015] The present invention is a method for preparing spherical micro-nano silicon dioxide by using a metal silicon powder deflagration method, wherein the metal silicon powder is cut from a metal silicon block to obtain the metal silicon powder, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by the combustion of a combustible gas and oxygen under the protection of an inert gas to deflagrate, react with oxygen to form silicon dioxide, and melt at high temperature to prepare the spherical micro-nano silicon dioxide. The present invention avoids the problem that high-temperature molten silicon in a slurry method is easily oxidized and heating pure oxygen is unsafe, and at the same time, the obtained spherical silicon dioxide has a more stable structure and is melted more thoroughly. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a TEM morphology image of spherical micro-nano silica in Example 1;

[0017] Figure 2 This is the TEM morphology of spherical micro-nano silica in Example 2;

[0018] Figure 3 This is the TEM morphology of spherical micro-nano silica in Example 3;

[0019] Figure 4 is a TEM morphology image of spherical micro-nano silica in Example 4;

[0020] Figure 5 is a TEM morphology image of spherical micro-nano silica in Example 5;

[0021] Figure 6 is a TEM morphology image of spherical micro-nano silica in Example 6;

[0022] Figure 7 is a TEM morphology image of spherical micro-nano silica in Example 7;

[0023] Figure 8 This is a TEM morphology image of spherical micro-nano silica in Example 8;

[0024] Fig. 9 This is the TEM morphology of the spherical micro-nano silica of Example 9. DETAILED DESCRIPTION

[0025] In order to make the technical problems, technical solutions and comparative effects to be solved by the present invention clearer, the present invention is further described in detail in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] In the following description, for the purpose of illustration rather than limitation, many specific details of internal procedures, techniques, etc. are provided to provide a thorough explanation of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention can be implemented in other embodiments without these specific details. In this embodiment, the description of the well-known capture system, gas supply device, circuit, etc. is omitted to avoid unnecessary details that hinder the description of the present invention.

[0027] The D50 particle size of the metallic silicon powder used in the following examples is less than or equal to 1 micron, and the D10 particle size is greater than or equal to 0.5 micron.

[0028] Example 1

[0029] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by natural gas and oxygen at a temperature of 2200 degrees by nitrogen for deflagration, wherein the feeding amount of the metal silicon powder when introduced into the high-temperature flame is 360 kg / hour, the nitrogen supply is set to 50 cubic meters / hour, the oxygen supply is set to 700 cubic meters / hour, and the natural gas supply is set to 360 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0030] Example 2

[0031] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by natural gas and oxygen at a temperature of 2400 degrees for explosion. The feeding amount of the metal silicon powder when introduced into the high-temperature flame is 380 kg / hour, the nitrogen supply is set to 60 cubic meters / hour, the oxygen supply is set to 720 cubic meters / hour, and the natural gas supply is set to 400 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0032] Example 3

[0033] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by acetylene and oxygen at a temperature of 2000 degrees for deflagration. The feeding amount of the metal silicon powder when introduced into the high-temperature flame is 350 kg / hour, the nitrogen supply is set to 40 cubic meters / hour, the oxygen supply is set to 680 cubic meters / hour, and the acetylene supply is set to 350 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0034] Example 4

[0035] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by acetylene and oxygen at a temperature of 2400 degrees for deflagration. The feeding amount of the metal silicon powder when introduced into the high-temperature flame is 360 kg / hour, the nitrogen supply is set to 60 cubic meters / hour, the oxygen supply is set to 700 cubic meters / hour, and the acetylene supply is set to 380 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0036] Example 5

[0037] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by natural gas and oxygen at a temperature of 2300 degrees for explosion by nitrogen, wherein the feeding amount of the metal silicon powder when introduced into the high-temperature flame is 370 kg / hour, the nitrogen supply is set to 50 cubic meters / hour, the oxygen supply is set to 700 cubic meters / hour, and the natural gas supply is set to 380 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0038] Example 6

[0039] The metal silicon block is cut into metal silicon powder with a particle size of 1000 nanometers, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by acetylene and oxygen at a temperature of 2350 degrees for deflagration. The feeding amount of the metal silicon powder when introduced into the high-temperature flame is 380 kg / hour, the nitrogen supply is set to 50 cubic meters / hour, the oxygen supply is set to 700 cubic meters / hour, and the acetylene supply is set to 360 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0040] Example 7

[0041] The metal silicon block is cut into metal silicon powder with a particle size of 1000, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by acetylene and oxygen at a temperature of 2400 degrees by nitrogen for deflagration, wherein the feeding amount of the metal silicon powder when introduced into the high-temperature flame is 370 kg / hour, the nitrogen supply is set to 60 cubic meters / hour, the oxygen supply is set to 720 cubic meters / hour, and the acetylene supply is set to 390 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0042] Example 8

[0043] The metal silicon block is cut into metal silicon powder with a particle size of 1000, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by natural gas and oxygen at a temperature of 2350 degrees by nitrogen for deflagration, wherein the feeding amount of the metal silicon powder when introduced into the high-temperature flame is 355 kg / hour, the nitrogen supply is set to 55 cubic meters / hour, the oxygen supply is set to 680 cubic meters / hour, and the natural gas supply is set to 390 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0044] Example 9

[0045] The metal silicon block is cut into metal silicon powder with a particle size of 1000, and then the metal silicon powder is uniformly introduced into a high-temperature flame of 2150 degrees formed by natural gas, acetylene and oxygen by nitrogen for deflagration, wherein the feeding amount of the metal silicon powder when introduced into the high-temperature flame is 375 kg / hour, the nitrogen supply is set to 45 cubic meters / hour, the oxygen supply is set to 690 cubic meters / hour, and the natural gas and acetylene supply are set to 380 cubic meters / hour to produce silicon dioxide. After high-temperature melting, spherical micro-nano silicon dioxide is prepared.

[0046] The morphology of spherical micro-nano silica was observed using a transmission electron microscope.

[0047] As can be seen from the figure, the prepared spherical micro-nano silica has good sphericity and has no safety hazards during the preparation process, and can be widely used.

[0048] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing spherical micro-nano silicon dioxide by using a metallic silicon powder deflagration method, characterized in that: The preparation method is as follows: a metal silicon block is cut into metal silicon powder, and then the metal silicon powder is uniformly introduced into a high-temperature flame formed by a combustible gas and oxygen by an inert gas to cause deflagration to produce silicon dioxide, and after high-temperature melting, spherical micro-nano silicon dioxide is prepared; In the step, the D50 particle size of the cut metal silicon powder is less than or equal to 1 micron, the D10 particle size is greater than or equal to 0.5 micron, and the particle size of the metal silicon powder is 1000 nanometers; In the steps, the inert gas is nitrogen, and the combustible gas is one or two of natural gas and acetylene; In the step, the feeding amount of the metallic silicon powder when the cyclone is uniformly introduced into the high-temperature flame is 350-380 kg / hour; In the steps, the supply amount of the inert gas is set to 40-60 cubic meters per hour; In the steps, the oxygen supply is set to 650-720 cubic meters per hour; In the steps, the supply volume of the combustible gas is set to 350-400 cubic meters per hour; In the steps, the temperature of the high-temperature flame formed by the combustion of the combustible gas and oxygen during the deflagration process is 2000-2400 degrees.

Citation Information

Patent Citations

  • Method for preparing spherical silicon dioxide by deflagration of slurry

    CN114560469A

  • Preparation method of nanoscale spherical silicon dioxide powder

    CN116332191A

  • Production of silicon dioxide powder

    JP1992132610A

  • Method for manufacturing ultrafine powder silica

    JP2001354409A

  • Fine spheroidal silica powder manufacturing method

    JP2002167214A