Synthesis and application of nano oil-displacing agent mediated by Bacillus subtilis BC23
The microbial-based nano-oil displacing agent combined with the fermentation of Bacillus subtilis strain BC23 and metal ions has solved the problems of low oil production efficiency and environmental pollution in oil fields, and achieved high-efficiency and low-cost nano-oil displacement effects.
Patent Information
- Application Number
- CN202410073863.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-01-18
AI Technical Summary
The existing technology lacks microbial agents specifically used to prepare nano-oil displacing agents, resulting in low oil production efficiency in oil fields, and traditional nanomaterial synthesis methods have problems with environmental pollution and high costs.
The fermentation liquid of Bacillus subtilis strain BC23 is mixed with silver ions and zinc ions, and through the preparation of microbial-based composite nano-oil displacing agent, its surfactant and emulsifier components are used to reduce the liquid surface tension and promote the emulsification and oil displacement process of crude oil.
It improves the oil recovery rate, reduces the oil-water interfacial tension, enhances the stability and dispersion of nanoparticles, reduces environmental pollution, has low cost, and is suitable for oil field production.
Smart Images

Figure CN117903985B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microbial oil displacement, and specifically relates to Bacillus subtilis BC23-mediated synthesis of a nano oil displacement agent and application thereof. Background Art
[0002] Nanoparticles have small unit sizes and large specific surface areas. Nanomaterials can be used to improve oil recovery. Nanoparticles can be dispersed in water or oil-water mixed systems to drive oil alone, or they can be used in combination with surfactants or polymers. According to the state of existence of nano oil-displacing agents, they are divided into nano powders, nano Pickering emulsions, and nano emulsions. Nanomaterials can be used to prepare nano oil-displacing agents through modification, configuration of emulsion systems, etc., and can be used in oilfield operations to achieve good results.
[0003] Nanomaterial synthesis methods can be divided into physical methods, chemical methods and biological methods. Physical methods use mechanical pressure, high-energy radiation, heat or electrical energy to wear, melt, evaporate or condense materials to produce nanoparticles. These methods mainly adopt a top-down strategy, which has the advantage of not being contaminated by solvents and producing uniform monodisperse NPs. The disadvantage is also very obvious, that is, the large amount of waste generated during the synthesis process makes physical synthesis costly. Chemical synthesis methods can achieve control of material size and shape by optimizing the synthesis process, the transformation mechanism of precursors, surface stabilizers and reagents in the system and their correlation with growth and nucleation rates. However, chemical methods are generally more dangerous and involve the use of toxic solvents, which do not meet the requirements of green chemistry. Therefore, the use of new eco-friendly agents instead of chemical agents to reduce risks and the use of green and environmentally friendly biological methods to achieve non-toxic nanoparticle synthesis methods have broad development potential. However, there is currently a lack of microbial agents specifically used for the preparation of nanoparticles as oil displacement agents, and there is an urgent need to find microbial agents that can be used specifically for oil displacement and improve oil recovery. Summary of the invention
[0004] In view of the defects in the prior art, the purpose of the present invention is to provide a microbial agent that can be used specifically for preparing an oil-displacing agent to improve the recovery rate of crude oil by the oil-displacing agent.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] The invention provides a Bacillus subtilis strain BC23, and the preservation number of the strain BC23 is: CCTCC NO.M2023700.
[0007] Preferably, the 16S rRNA nucleotide sequence of the strain BC23 is as shown in SEQ ID NO.1.
[0008] The present invention provides a fermentation broth of the Bacillus subtilis strain BC23 described in the above technical solution.
[0009] The present invention provides a method for preparing the fermentation solution described in the above technical solution, comprising the following steps:
[0010] The Bacillus subtilis strain BC23 is cultured in a culture medium to obtain a fermentation solution.
[0011] The present invention provides the use of the Bacillus subtilis strain BC23 described in the above technical solution, the fermentation solution described in the above technical solution or the fermentation solution prepared by the preparation method described in the above technical solution in preparing nanoparticle materials.
[0012] The present invention provides the use of the Bacillus subtilis strain BC23 described in the above technical solution, the fermentation solution described in the above technical solution or the fermentation solution prepared by the preparation method described in the above technical solution in the preparation of an oil displacement agent.
[0013] The present invention provides a microbial-based composite nano oil-displacing agent, comprising: bimetallic nanoparticles and the fermentation bacterial solution described in the above technical solution; the bimetallic nanoparticles comprise nanosilver and nanozinc oxide.
[0014] The present invention provides a method for preparing the microbial-based composite nano oil-displacing agent described in the above technical solution, comprising the following steps:
[0015] mixing the silver ion solution and the zinc ion solution to obtain a metal precursor solution;
[0016] The metal precursor solution is mixed with the fermentation bacterial solution and then cultured to obtain a microbial-based composite nano oil-displacing agent.
[0017] Preferably, the molar concentration ratio of silver ions to zinc ions in the metal precursor solution is (0.25-0.75): (0.25-0.75);
[0018] The volume ratio of the metal precursor solution to the fermentation liquid is (1-3):(1-3);
[0019] The culture temperature is 35°C to 37°C;
[0020] The culture time is 12 to 48 hours.
[0021] The present invention provides the use of the microbial-based composite nano oil-displacing agent described in the above technical solution or the microbial-based composite nano oil-displacing agent prepared by the preparation method described in the above technical solution in oil field production and / or improving crude oil recovery.
[0022] Beneficial effects of the present invention:
[0023] The present invention provides a Bacillus subtilis strain BC23, and the deposit number of the strain BC23 is: CCTCC NO.M2023700. The Bacillus subtilis strain BC23 provided by the present invention is fermented and cultured to obtain a fermented bacterial liquid. The surfactant and emulsifier components contained in the fermented bacterial liquid can reduce the surface tension of the liquid, emulsify the crude oil, and promote the oil displacement process. The fermented bacterial liquid can be used as a reducing agent and stabilizer for nanoparticles and / or bimetallic nanoparticles, prevent the nanoparticles and / or bimetallic nanoparticles from aggregating, and achieve uniform dispersion of the nanoparticles and / or bimetallic nanoparticles. The nanoparticles and / or bimetallic nanoparticles prepared by the fermented bacterial liquid have a small particle size, can greatly reduce the oil-water interfacial tension, are more likely to displace the crude oil in the pores, have a temporary blocking effect on small pores, and improve the recovery rate by expanding the sweep efficiency; the nanoparticles and / or bimetallic nanoparticles can also change the wettability of the reservoir, and increase the influence of the surfactant on the oil recovery process. In summary, the Bacillus subtilis strain BC23 provided by the present invention can be used exclusively for preparing oil displacement agents to improve the recovery rate of oil displacement agents. The Bacillus subtilis strain BC23 provided by the present invention has broad application prospects in the field of oil and natural gas collection.
[0024] Furthermore, the fermentation broth of the Bacillus subtilis strain BC23 of the present invention can be used as a reducing agent and stabilizer for nanoparticles and / or bimetallic nanoparticles to prevent the aggregation of nanoparticles and / or bimetallic nanoparticles, achieve uniform dispersion of nanoparticles and / or bimetallic nanoparticles, and be used to prepare nanoparticles and / or bimetallic nanoparticles. The nanoparticles and / or bimetallic nanoparticles prepared by the Bacillus subtilis strain BC23 or the fermentation broth of the present invention have high stability and small particle size. The bimetallic nanoparticles prepared by the Bacillus subtilis strain BC23 or the fermentation broth of the present invention can achieve a synergistic technical effect in the catalytic reduction of metals.
[0025] Furthermore, the fermentation liquid of the Bacillus subtilis strain BC23 of the present invention can be reacted with metal ions to prepare a microbial-based nano oil-displacing agent. The fermentation liquid of the Bacillus subtilis strain BC23 of the present invention is mixed with silver ions and zinc ions and then cultured to prepare a microbial-based composite nano oil-displacing agent; the microbial-based composite nano oil-displacing agent can be applied to oil field production to improve crude oil recovery. The microbial-based composite nano oil-displacing agent provided by the present invention is applied to the collection of crude oil in oil fields, which can effectively improve the recovery rate.
[0026] Biological Deposit Description
[0027] Bacillus subtilis strain BC23 was deposited in the China Center for Type Culture Collection CCTCC on May 8, 2023, with the deposit address: Wuhan University, Wuhan, China, and the deposit number is: CCTCC NO.M2023700. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0029] Figure 1 This is a photo of the colonies of Bacillus subtilis BC23 strain on LB plate;
[0030] Figure 2 This is an electron microscopic photograph of Bacillus subtilis BC23 strain;
[0031] Figure 3 This is the 16S rRNA evolutionary tree of Bacillus subtilis BC23 strain;
[0032] Figure 4 Schematic diagram of the emulsification effect of Bacillus subtilis BC23 strain;
[0033] Figure 5 The effect diagram of the microbial-based composite nano oil-displacing agent prepared in Examples 4 to 12;
[0034] Figure 6 This is a graph showing the results of laser particle size analyzer testing of bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent prepared in Example 10;
[0035] Figure 7 This is an X-ray energy spectrum electron diagram of the bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent prepared in Example 10;
[0036] Figure 8 This is an elemental composition diagram of the bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent prepared in Example 10 obtained by X-ray energy spectrometer;
[0037] Fig. 9 This is a scanning electron microscope image of the bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent prepared in Example 10;
[0038] Fig.10FTIR spectra of microbial agents and microbial-based composite nano-oil-displacing agents;
[0039] Fig.11 The graph of the change in contact angle of the J-1 and J-2 test groups in the oil-water-solid three-phase system in Example 19;
[0040] Fig.12 The graph of the change in contact angle of the J-3 and J-4 test groups in the oil-water-solid three-phase system in Example 19;
[0041] Fig.13 The graph of the change in contact angle of the J-5 and J-6 test groups in the oil-water-solid three-phase system in Example 19;
[0042] Fig.14 The graph of the change in contact angle of the J-7 and J-8 test groups in the oil-water-solid three-phase system in Example 19;
[0043] Fig.15 This is a graph showing the results of a microscopic oil displacement experiment of the microbial-based composite nano-oil displacement agent synthesized in Example 10. DETAILED DESCRIPTION
[0044] The invention provides a Bacillus subtilis strain BC23, and the preservation number of the strain BC23 is: CCTCC NO.M2023700.
[0045] In the present invention, the Bacillus subtilis strain BC23 is isolated from an oilfield water sample. In the present invention, the Bacillus subtilis strain BC23 was deposited in the China Center for Type Culture Collection on May 8, 2023, with a deposit number of CCTCC NO.M2023700.
[0046] In the present invention, the Bacillus subtilis strain BC23 is grown in solid LB medium for 24 hours, and the colony morphology is circular with extremely irregular edges, the surface is moist and wrinkled, and it is milky white. In the present invention, the results of scanning electron microscopy observation of the Bacillus subtilis strain BC23 bacteria show that the bacteria are rod-shaped and the spores are short rod-shaped. In the present invention, the growth temperature range of the Bacillus subtilis strain BC23 is preferably 35°C to 37°C, more preferably 37°C; the pH tolerance value of the Bacillus subtilis strain BC23 is preferably 7.0 to 7.5, more preferably 7.0.
[0047] In the present invention, the Bacillus subtilis strain BC23 can secrete a surfactant component to reduce surface tension. The Bacillus subtilis strain BC23 of the present invention can secrete an emulsifier component. The present invention proves through experiments that the Bacillus subtilis strain BC23 bacterial agent can reduce surface tension, thereby proving that the Bacillus subtilis strain BC23 can secrete a surfactant component. The present invention shows through experiments that the Bacillus subtilis strain BC23 bacterial agent has a strong emulsifying effect, and has a significant emulsifying effect on both liquid oil and block oil, proving that the Bacillus subtilis strain BC23 of the present invention can secrete an emulsifier component, thereby enabling its fermented bacterial liquid to emulsify oil.
[0048] In the present invention, the nucleotide sequence of 16S rRNA of the Bacillus subtilis strain BC23 is 1412 bp in total, as shown in SEQ ID NO.1.
[0049] The 16S rRNA nucleotide sequence of Bacillus subtilis strain BC23 obtained in the present invention was compared with the NCBI database to construct a phylogenetic tree. Figure 3 The similarity between strain BC23 and Bacillus subtilis is close to 100%, and strain BC23 can be identified as Bacillus subtilis.
[0050] The present invention provides a fermentation broth of the Bacillus subtilis strain BC23 described in the above technical solution. In the present invention, the fermentation broth contains an emulsifier component and a surfactant component.
[0051] The present invention provides a method for preparing the fermentation solution described in the above technical solution, comprising the following steps:
[0052] The Bacillus subtilis strain BC23 is cultured in a culture medium to obtain a fermentation solution.
[0053] In the present invention, the culture medium is preferably a fermentation medium; the composition of the fermentation medium preferably includes the following raw materials in percentage by weight: C6H 12 O61.0%~1.5%, Na2SO40.2%~0.5%, K2HPO4·3H2O 0.2%~0.5%, NH4Cl 0.1%~0.2%, MgCl2·6H2O 0.02%~0.06%, sodium lactate 0.2%~0.4%, and the balance is deionized water, and the sum of the mass percentages of the above components is 100%. In the present invention, the composition of the fermentation medium preferably includes the following raw materials in mass percentage: C6H 12O61.0%, Na2SO40.2%, K2HPO4·3H2O 0.2%, NH4Cl 0.1%, MgCl2·6H2O 0.03%, sodium lactate 0.2%, and the remainder is deionized water. The sum of the mass percentages of the above components is 100%. In the present invention, the pH of the fermentation medium is preferably 7.0-7.5, and more preferably 7.0. The culture temperature of the present invention is preferably 35°C-37°C, more preferably 36°C-37°C, and more preferably 37°C; the culture time is preferably 3-7d, more preferably 3-5d, more preferably 3-4d, and most preferably 3d. The culture of the present invention is preferably carried out in a shaker, and the rotation speed of the shaker is preferably 150-300rpm, and more preferably 180rpm.
[0054] In the present invention, the viable count of the fermentation broth is preferably OD 600 The fermentation liquid has a value of 0.8 to 1.0. The fermentation liquid is proved to contain emulsifier and surfactant components by measuring the surface tension and emulsification ability of the fermentation liquid. In the present invention, the fermentation liquid preferably contains aromatic and aliphatic substances.
[0055] The present invention provides the use of the Bacillus subtilis strain BC23 described in the above technical solution, the fermentation solution described in the above technical solution, or the fermentation solution prepared by the preparation method described in the above technical solution in the preparation of nanoparticle materials. In the present invention, the nanoparticle material preferably includes monometallic nanoparticles and / or bimetallic nanoparticles, more preferably bimetallic nanoparticles. The Bacillus subtilis strain BC23 or the fermentation solution described in the present invention can preferably be used to prepare nanoparticles and / or bimetallic nanoparticles. The fermentation solution of the Bacillus subtilis strain BC23 described in the present invention can be used as a reducing agent and stabilizer for nanoparticles and / or bimetallic nanoparticles to prevent the aggregation of nanoparticles and / or bimetallic nanoparticles and achieve uniform dispersion of nanoparticles and / or bimetallic nanoparticles. The nanoparticles and / or bimetallic nanoparticles prepared by the Bacillus subtilis strain BC23 or the fermentation solution described in the present invention have high stability and small particle size. The bimetallic nanoparticles prepared by the Bacillus subtilis strain BC23 or the fermentation solution described in the present invention can achieve a synergistic technical effect in catalytic reduction of metals and oil displacement.
[0056] The present invention provides the use of the Bacillus subtilis strain BC23 described in the above technical solution, the fermentation solution described in the above technical solution, or the fermentation solution prepared by the preparation method described in the above technical solution in the preparation of an oil-displacing agent. In the present invention, the oil-displacing agent preferably includes a microbial-based composite nano oil-displacing agent. The Bacillus subtilis strain BC23 or the fermentation solution described in the present invention can be compounded with nanoparticles and / or bimetallic nanoparticles for use as a microbial-based nano oil-displacing agent. The Bacillus subtilis strain BC23 or the fermentation solution described in the present invention can also react with metal ions to prepare a microbial-based nano oil-displacing agent. In the present invention, the microbial-based nano oil-displacing agent is applied to oilfield operations, which can greatly improve the recovery rate while reducing pollution to the natural environment and secondary damage to the reservoir.
[0057] The present invention provides a microbial-based composite nano oil-displacing agent, comprising: bimetallic nanoparticles and the fermentation bacterial solution described in the above technical solution; the bimetallic nanoparticles comprise nanosilver and nanozinc oxide.
[0058] In the present invention, the microbial-based composite nano oil-displacing agent is preferably obtained by mixing the fermentation solution and the metal precursor solution in the above technical solution and then culturing. In the present invention, the preparation method of the fermentation solution has been recorded in the above technical solution and will not be repeated here; the metal precursor solution is preferably composed of silver ions and zinc ions. In the present invention, the molar concentration ratio of zinc ions and silver ions in the metal precursor solution is preferably (0.25-0.75): (0.25-0.75), more preferably (0.25-0.5): (0.5-0.75), and more preferably 0.25: 0.75. In the present invention, the volume ratio of the metal precursor solution and the fermentation solution is preferably (1-3): (1-3), more preferably (1-3): 1, more preferably (1-2): 1, and more preferably 1: 1. In the present invention, the metal precursor solution is mixed with the fermentation solution and then cultured; the culture temperature is preferably 35°C to 37°C; the culture time is preferably 12 to 48h. The preparation method of the microbial-based composite nano oil-displacing agent prepared by using fermented bacterial liquid and metal precursors is described in detail below and will not be repeated here.
[0059] In the present invention, the bimetallic nanoparticles preferably include nanosilver and nanozinc oxide; the particle size of the bimetallic nanoparticles is preferably 20 to 100 nm, more preferably 20 to 50 nm, and more preferably 37 nm; the bimetallic nanoparticles are preferably in the form of a fluid in the fermentation broth. In the present invention, the bimetallic nanoparticles have the advantages of uniform shape and small particle size, and have a larger surface energy that is conducive to full contact with crude oil, providing a more excellent effect of enhancing crude oil recovery.
[0060] The present invention provides a method for preparing the microbial-based composite nano oil-displacing agent described in the above technical solution, comprising the following steps:
[0061] mixing the silver ion solution and the zinc ion solution to obtain a metal precursor solution;
[0062] The metal precursor solution is mixed with the fermentation bacterial solution and then cultured to obtain a microbial-based composite nano oil-displacing agent.
[0063] The present invention mixes a silver ion solution and a zinc ion solution to obtain a metal precursor solution.
[0064] In the present invention, the molar concentration ratio of zinc ions and silver ions in the metal precursor solution is preferably (0.25-0.75): (0.25-0.75), further preferably (0.25-0.5): (0.5-0.75), and more preferably 0.25: 0.75. In the present invention, the molar concentration of zinc ions in the metal precursor solution is preferably 0.25-0.75 mmol / L, and the molar concentration of silver ions is preferably 0.25-0.75 mmol / L; further preferably, the molar concentration of zinc ions is preferably 0.25-0.5 mmol / L, and the molar concentration of silver ions is preferably 0.5-0.75 mmol / L; more preferably, the molar concentration of zinc ions is preferably 0.25 mmol / L, and the molar concentration of silver ions is preferably 0.75 mmol / L. The present invention does not specifically limit the sources of silver ions and zinc ions, and conventional silver ion reagents and zinc ion reagents in the art can be used. The present invention does not specifically limit the configuration of silver ion solutions and zinc ion solutions, and conventional solution configuration methods in the art can be used. In the present invention, the metal precursor solution preferably does not contain chloride ions, otherwise the reducing ability of the fermentation broth is insufficient to replace the elemental metal particles. In the present invention, the zinc ion solution preferably includes a hexahydrate zinc acetate solution; the silver ion solution preferably includes a silver nitrate solution. The molar concentration ratio of silver ions to zinc ions in the metal precursor solution of the present invention is conducive to the reasonable configuration of the prepared nano silver element and nano zinc oxide element, and helps to obtain bimetallic nanoparticles with smaller particle sizes.
[0065] After obtaining the metal precursor solution, the present invention mixes the metal precursor solution with the fermentation bacterial solution described in the above technical solution and then cultures them to obtain a microbial-based composite nano oil-displacing agent.
[0066] In the present invention, the volume ratio of the metal precursor solution and the fermentation broth is preferably (1-3): (1-3), more preferably (1-3): 1, more preferably (1-2): 1, and more preferably 1: 1. In the present invention, the ratio of the metal precursor solution and the fermentation broth is conducive to obtaining bimetallic nanoparticles with smaller particle size. The method of mixing the metal precursor solution and the fermentation broth in the present invention is preferably to add the metal precursor solution to the Bacillus subtilis broth in a sterile environment; the process of adding the metal precursor solution to the Bacillus subtilis broth must be strictly operated in a sterile clean bench to prevent contamination. After the metal precursor solution is mixed with the fermentation broth in the above technical solution, the mixed solution is preferably cultured; the culture temperature is preferably 35°C to 37°C, more preferably 37°C; the culture time is preferably 12 to 48h, more preferably 12 to 24h, more preferably 24h; the culture is preferably carried out in a shaker; the rotation speed of the shaker is preferably 150 to 300rpm, more preferably 180rpm. After the cultivation is completed, the obtained white precipitate is the crude product of the microbial-based composite nano oil-displacing agent.
[0067] After obtaining the crude microbial-based composite nano oil-displacing agent, the present invention preferably purifies the crude microbial-based composite nano oil-displacing agent to obtain the microbial-based composite nano oil-displacing agent. The purification method of the present invention preferably uses a 0.22 μm vacuum filter membrane to filter the crude oil-displacing agent to remove bacterial interference, then centrifuges at 8000 rpm, 5 min, discards the supernatant, adds an appropriate amount of deionized water and shakes, then centrifuges and discards the supernatant, and repeats the cycle three times to obtain a relatively pure microbial-based composite nano oil-displacing agent. The relatively pure composite nano oil-displacing agent can also be further dried to obtain a solid microbial-based composite nano oil-displacing agent.
[0068] In the present invention, the microbial-based composite nano oil-displacing agent is a liquid preparation. The microbial-based composite nano oil-displacing agent of the present invention can also be a solid preparation. When the microbial-based composite nano oil-displacing agent is a solid preparation, the present invention preferably dries the liquid preparation of the microbial-based composite nano oil-displacing agent to obtain a solid preparation; the drying method is preferably vacuum freeze drying or low-temperature drying. In the present invention, the temperature of the low-temperature drying is preferably 60°C. When the microbial-based composite nano oil-displacing agent of the present invention is in the form of a solid preparation, it can be dispersed in water and directly applied to oilfield oil displacement.
[0069] The microbial-based composite nano oil-displacing agent prepared by the preparation method of the microbial-based composite nano oil-displacing agent provided by the present invention is a simple method for synthesizing a composite nano oil-displacing agent, and compared with the previous technology, it has the advantages of obvious recovery effect, wide source of raw materials, and low cost. The effect of improving the recovery rate of the microbial-based composite nano oil-displacing agent of the present invention is linearly correlated with the concentration of the microbial-based composite nano oil-displacing agent. The bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent obtained by the preparation method of the present invention have the advantages of uniform shape and small particle size, and have a larger surface energy that is conducive to full contact with crude oil, providing a more excellent effect of improving the recovery rate.
[0070] The present invention provides the application of the microbial-based composite nano oil-displacing agent described in the above technical solution in oil field oil production and / or improving oil recovery. In the present invention, the fermented bacterial liquid in the microbial-based composite nano oil-displacing agent contains surfactants and emulsifier components, mainly aromatic and aliphatic substances, which can reduce the surface tension of the liquid, emulsify the crude oil, and promote the oil recovery process. The bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent have a small particle size, which can greatly reduce the oil-water interfacial tension and make it easier to displace the crude oil in the pores. At the same time, the bimetallic nanoparticles have a temporary blocking effect on small pores, and improve the recovery rate by expanding the sweep efficiency; the bimetallic nanoparticles can change the wettability of the reservoir and increase the influence of the surfactant solution on the oil recovery process. The results of the examples show that the microbial-based composite nano oil-displacing agent provided by the present invention can reduce the contact angle of the crude oil-nanofluid system and improve the wettability of the reservoir rock. The microbial-based composite nano oil-displacing agent can penetrate into more complex and finer formation pores to play a role, and improve the oil recovery effect significantly.
[0071] In order to further illustrate the present invention, the technical solution provided by the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0072] Example 1
[0073] 1. Screening of Bacillus subtilis strain BC23
[0074] Take the wastewater sample of Changqing Oilfield, add 10wt.% crude oil, 0.5wt.% peptone and 0.35wt.% ammonium chloride to the water sample, and culture at 37℃, 180rpm for 5-7 days. Dilute the culture solution by gradient 10 -4 , 10 -5 , 10 -6 Spread on LB plate, continue to culture for 24 hours, pick single colonies of different morphologies, and inoculate them into fermentation medium after high temperature sterilization. Observe the strains that have emulsification effect on crude oil, name one of them as strain BC23, save the strain BC23 sample for the next step of identification and analysis.
[0075] The fermentation medium used above is composed of the following raw materials in percentage by mass: C6H 12 O61.0%, Na2SO40.2%, K2HPO4·3H2O 0.2%, NH4Cl 0.1%, MgCl2·6H2O 0.03%, sodium lactate 0.2%, the balance is deionized water, the sum of the mass percentages of the above components is 100%. Use 0.1M NaOH solution and 0.1M HCl solution to adjust the pH to 7.0.
[0076] 2. Identification of strain BC23
[0077] (1) Morphological observation of strain BC23
[0078] The strain BC23 was cultured on solid LB medium at 37°C for 24 h and the colony morphology of the strain was observed. Figure 1 The bacteria were examined by scanning electron microscopy, and the results were as follows Figure 2 shown.
[0079] Depend on Figure 1 and Figure 2 It was found that the colonies of strain BC23 grown in solid LB medium for 24 hours were circular with irregular edges, moist and wrinkled surface, and milky white. The results of scanning electron microscopy showed that the bacteria were rod-shaped and the spores were short rod-shaped.
[0080] By further culturing the strain, it was finally determined that the suitable growth temperature range of strain BC23 was 35℃~37℃, and the pH tolerance was 7~7.5.
[0081] (2) Molecular identification
[0082] The DNA barcode fragment corresponding to strain BC23 was amplified by colony PCR, and its DNA sequence was obtained using the gold standard sequencing method - Sanger sequencing. The 16S rRNA sequence of strain BC23 was obtained as shown in SEQ ID NO.1, specifically:
[0083]
[0084] The 16S rRNA was compared and analyzed in the NCBI database. Generally, if the sequence similarity is more than 97%, it can be considered to be the same species. The phylogenetic tree based on the 16S rRNA gene sequence is as follows: Figure 3 . Figure 3 The BSU in the expression refers to strain BC23, which has a similarity of nearly 100% with Bacillus subtilis, and can be identified as Bacillus subtilis.
[0085] Through morphological characteristics and molecular biology 16S rRNA gene sequencing identification results, strain BC23 was identified as Bacillus subtilis.
[0086] Example 2
[0087] Preparation of Bacillus subtilis BC23 inoculant (also referred to as fermentation liquid of Bacillus subtilis BC23)
[0088] Bacillus subtilis BC23 is inoculated into a fermentation medium for shaking culture to obtain a Bacillus subtilis BC23 bacterial agent.
[0089] The fermentation medium consists of the following raw materials in percentage by weight: C6H 12 O61.0%, Na2SO40.2%, K2HPO4·3H2O 0.2%, NH4Cl 0.1%, MgCl2·6H2O 0.03%, sodium lactate 0.2%, the balance is deionized water, the sum of the mass percentages of the above components is 100%. Use 0.1M NaOH solution and 0.1M HCl solution to adjust the pH to 7.0.
[0090] The shaking incubation temperature was 37°C; the shaking incubation time was 4 days; and the shaking speed was 180 rpm.
[0091] After the shaking culture is completed, a Bacillus subtilis BC23 inoculum (also referred to as a fermentation broth of Bacillus subtilis BC23) is obtained, with an OD600nm value of 0.8-1.
[0092] Example 3
[0093] The surface tension and emulsification performance test of Bacillus subtilis BC23 inoculant (also known as the fermentation solution of Bacillus subtilis BC23) are as follows:
[0094] 1. Surface tension measurement
[0095] The platinum sheet was burned to red with the outer flame of an alcohol lamp, and the tension meter was zeroed after cooling to room temperature. The surface tension meter was zeroed to 72mN / m using deionized water. The platinum sheet was slowly contacted with the surface of the liquid to be tested. The liquid to be tested here refers to the Bacillus subtilis BC23 inoculum prepared in Example 2. The surface tension of the liquid will pull the platinum sheet down. When the test value is stable, the surface tension of the sample is recorded as 43.3mN / m. Compared with the initial surface tension of 72mN / m of the surface tension meter, the surface tension is reduced, which indicates that the Bacillus subtilis BC23 inoculum contains surfactant components.
[0096] 2. Emulsification Determination
[0097] (1) Add 4 mL of kerosene to two 10 mL centrifuge tubes respectively, and drop 1 mL of the Bacillus subtilis BC23 inoculum prepared in Example 2 into one of the centrifuge tubes, shake evenly, and observe the emulsion layer after standing for 12 hours. Figure 4 As shown in A and B. Figure 4 A in the figure is the result of the control test without adding microbial agents. Figure 4 B in the figure is the result of the test with the addition of Bacillus subtilis BC23.
[0098] Depend on Figure 4 It can be seen that the centrifuge tube without adding Bacillus subtilis BC23 inoculant is clear and has no stratification, while the centrifuge tube with adding Bacillus subtilis BC23 inoculant has an obvious emulsified layer, indicating that Bacillus subtilis BC23 inoculant contains emulsifier components and can emulsify oil.
[0099] (2) Add 20 mL of deionized water and Bacillus subtilis BC23 to two 30 mL vials respectively, add an appropriate amount of block crude oil to each vial, shake thoroughly, and let stand for more than 48 hours to observe the emulsification phenomenon. Figure 4 As shown in C.
[0100] Depend on Figure 4 From C in the figure, it can be seen that Bacillus subtilis BC23 agent has an emulsifying effect on oil.
[0101] Embodiments 4 to 12
[0102] A method for preparing a microbial composite nano oil-displacing agent is as follows:
[0103] preparing a metal precursor solution containing silver ions and zinc ions at a certain molar concentration;
[0104] Under magnetic stirring conditions, the metal precursor solution is added to the Bacillus subtilis BC23 bacterial agent prepared in Example 2 in a certain volume ratio and mixed evenly, and the mixed solution of the metal precursor solution and the Bacillus subtilis BC23 bacterial agent is placed in a 37°C constant temperature shaker for a certain period of time to obtain a crude oil-displacing agent. The crude oil-displacing agent is filtered using a 0.22 μm vacuum filter membrane to remove bacterial interference, and then centrifuged using a high-speed centrifuge under the conditions of 8000rpm and 5min. After discarding the supernatant, an appropriate amount of deionized water is added and shaken, and then the supernatant is discarded by centrifugation. This cycle is repeated three times to obtain a relatively pure microbial-based composite nano oil-displacing agent. The microbial-based composite nano oil-displacing agent here can be used directly in the subsequent use, or it can be dried, specifically: dried at 60°C to obtain a microbial-based composite nano oil-displacing agent. The specific parameters of Examples 4 to 12 are shown in Table 1.
[0105] Table 1 Specific parameters for preparing microbial composite nano oil displacement agents in Examples 4 to 12
[0106]
[0107] The microbial-based composite nano oil-displacing agent prepared in Examples 4 to 12 is as follows Figure 5 shown. Figure 5 BSU-1 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 4, BSU-2 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 5, BSU-3 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 6, BSU-4 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 7, BSU-5 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 8, BSU-6 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 9, BSU-7 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 10, BSU-8 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 11, and BSU-9 corresponds to the microbial-based composite nano-oil-displacing agent prepared in Example 12.
[0108] Example 13
[0109] The particle sizes of the bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agents prepared in Examples 4 to 12 were detected using a laser particle size analyzer.
[0110] Detection method:
[0111] 1. Turn on the computer first, then turn on the instrument power switch, and preheat for about half an hour to stabilize the laser output power.
[0112] 2. Prepare a clean cuvette, clean the surface with alcohol, etc., and then dry it to ensure that there is no foreign matter on the surface. Then inject pure water into the cuvette, the height of the water surface is about 2 / 3 of the height of the cuvette, and note that the surface of the water must cover the position of the laser beam on the cuvette by 5mm.
[0113] 3. Open the sample chamber cover, place the cuvette filled with pure water into the fixed slot of the sample chamber, then remove the baffle in front of the detector, adjust the position of the cuvette so that the light spot reflected to the detector deviates slightly upwards, ensure that the reflected light spot does not shine on the receiving surface of the detector, and then cover the cover.
[0114] 4. Add samples and run the main program.
[0115] The particle sizes of the bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agents prepared in Examples 4 to 12 are shown in Table 2. The laser particle size analyzer test results of the microbial-based composite nano-oil-displacing agent prepared in Example 10 are shown in Table 2. Figure 6 shown.
[0116] Table 2 Particle size test results of bimetallic nanoparticles in the microbial-based composite nano oil-displacing agent prepared in Examples 4 to 12
[0117] Example serial number Average particle size (nm) Example 4 BSU-1 1966 Example 5 BSU-2 859 Example 6 BSU-3 48 Example 7 BSU-4 707 Example 8 BSU-5 56 Example 9 BSU-6 1764 Example 10 BSU-7 37 Embodiment 11 BSU-8 712 Example 12 BSU-9 1591
[0118] It can be seen from Table 2 that different conditions have different effects on the particle size of the bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agent. The degree of influence of different conditions on the particle size is as follows: metal ion concentration ratio> metal precursor to microbial volume ratio> reaction time. The particle size of the bimetallic nanoparticles in the microbial-based nano-oil-displacing agent prepared in Example 10 is the smallest, which is 37nm. In this example, the ratio of Ag atoms to Zn atoms is 1:1, which is preferably the optimal synthesis ratio. Figure 6 It can be obtained that the particle size of the bimetallic nanoparticles in the microbial-based nano oil-displacing agent prepared in Example 10 is mostly concentrated in the range of 20 to 50 nm. Since metal ions are easily aggregated and grown after being reduced to zero-valent metals, it is very important to find a suitable stabilizer to keep the particles at the nanometer level. The Bacillus subtilis agent used in the present invention contains a large number of macromolecular substances such as hydroxyl groups and carbonyl groups, which is conducive to the stable dispersion of bimetallic nanoparticles in the system.
[0119] Embodiment 14
[0120] The microbial-based composite nano oil-displacing agent prepared in Example 10 was detected using an X-ray energy spectrometer.
[0121] A very thin layer of gold was sprayed on the surface of the sample by vapor deposition to ensure that the sample has good conductivity. The EDX detector was connected to the SEM instrument (Oxford instruments). Energy dispersive X-ray spectroscopy was used to obtain the composition and elemental analysis of the bimetallic nanoparticles to determine the elemental composition of the bimetallic nanoparticles. The test results are shown in Figure 7 And as shown in Table 3.
[0122] Table 3 Elemental composition of bimetallic nanoparticles in microbial-based composite nano oil-displacing agent prepared in Example 10
[0123] element Wt% Wt%Sigma C 12.37 0.97 N 0.80 0.53 O 3.76 0.26 S 0.61 0.08 Cl 2.46 0.15 Zn 65.47 1.21 Ag 14.53 0.63
[0124] From Table 3 and Figure 7 It can be obtained that Ag (14.53%) and Zn (65.47%) exist in the Ag / ZnO bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agent system synthesized in Example 9. The reducibility of the Bacillus subtilis BC23 bacterial agent has the potential to synthesize bimetallic nanoparticles.
[0125] Embodiment 15
[0126] The surface morphology of the bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agent prepared in Example 10 was observed using a high-resolution Zeiss Merlin Compact scanning electron microscope at an accelerating voltage of 15 kV, with a magnification of 40 kX. The surface morphology of the bimetallic nanoparticles in the microbial-based composite nano-oil-displacing agent prepared in Example 10 is as follows: Figure 8 shown.
[0127] The morphology of the bimetallic nanoparticles was observed using a scanning electron microscope. Fig. 9 shown.
[0128] Depend on Figure 8 and Fig. 9 The image shows that the bimetallic nanoparticles are spherical and the particle size is about 40nm. The overall observation of the scanning image shows that the Bacillus subtilis inoculant extract can synthesize a bimetallic nanosystem with uniform shape and stable dispersion by reducing the metal salt solution.
[0129] Example 16
[0130] The samples were recorded using a ThermoScientific Nicolet 6700 FTIR infrared spectrometer at wavelengths (4000-400 cm -1) range is used to determine the specific material composition in the sample. The potassium bromide tablet method is used. Collect 1-2 mg of powder sample and 200 mg of pure KBr, grind them evenly, put them into a mold, and press them into transparent sheets on an oil press. Then, put the sample into an infrared spectrometer for testing. The wave number range is from 4000 to 400 cm -1 ; Scan times: 32 times, resolution: 4cm -1 .
[0131] Origin was used to draw the spectrum. The FTIR spectra of the Bacillus subtilis BC23 inoculum prepared in Example 2 and the bimetallic nanoparticles prepared in Example 10 were as follows: Fig.10 As shown. The infrared spectrum of Bacillus subtilis BC23 inoculant showed characteristic peaks at 3371, 2974, 1582, 1410, 1064, 861, 695, and 543. The infrared spectrum of Ag-ZnO NPs showed characteristic peaks at 3391, 2933, 1592, 1417, 1033, 1074, 771, 636, and 434 cm -1 The characteristic peak is shown at 3000cm. From the comparison of the two FTIR spectrum curves, it can be seen that the positions of the peaks are basically the same, and the intensities of the peaks detected at the same position are different. The difference in intensity may be related to the role played by the substance corresponding to the peak in the nanosynthesis process, or it may be related to the excited electrons. -1 The presence of an absorption peak indicates the presence of stretching vibration of unsaturated CH, which may be an alkene, alkyne, or aromatic compound; below 3000cm -1 The presence of absorption peaks indicates the presence of saturated CH stretching vibration absorption. For the bimetallic nanosample, the absorption peaks at 3391, 1592, and 1033 cm -1 The absorption peaks observed at 2933 and 1417 cm correspond to (OH) hydrogen bonds, (CO) and NH pulling vibrations, which can be preliminarily judged to be the presence of protein substances. -1 The peak at 772 cm is attributed to the CH stretching vibration and the COO-carboxyl side chain, while the peak at 772 cm -1 The peak at 1074 cm indicates that the OH plane is bent outward, which also indicates that aromatic and aliphatic substances may be involved, which may be attributed to the cell membrane of the bacteria. Negatively charged groups can interact with NPs through electrostatic interactions. Therefore, protein molecules metabolized by Bacillus subtilis can act as stabilizers for bimetallic nanoparticles. At the same time, the peak at 1074 cm -1 The characteristic peaks at indicate the presence of stretching vibration bands of aliphatic amine CN, while the amine bonds in proteins have strong metal binding ability. Therefore, the good dispersibility of the synthesized NPs may be due to the protein-coated bimetallic nanoparticles, which play a huge role in preventing the aggregation of nanoparticles and promoting the stability of nanoparticles in the culture medium.
[0132] Embodiment 17
[0133] The microbial-based composite nano oil-displacing agent stock solution prepared in Example 10 was diluted in a certain proportion and diluted with deionized water. The volume percentage of the microbial-based composite nano oil-displacing agent was 100%, recorded as N-12; the volume percentage of the microbial-based composite nano oil-displacing agent was 50%, recorded as N-11; the volume percentage of the microbial-based composite nano oil-displacing agent was 45%, recorded as N-10; the volume percentage of the microbial-based composite nano oil-displacing agent was 40%, recorded as N-9; the volume percentage of the microbial-based composite nano oil-displacing agent was 35%, recorded as N-8; the volume percentage of the microbial-based composite nano oil-displacing agent was 30%, recorded as N-7; the volume percentage of microbial-based composite nano oil-displacing agent is 25%, recorded as N-6; the volume percentage of microbial-based composite nano oil-displacing agent is 20%, recorded as N-5; the volume percentage of microbial-based composite nano oil-displacing agent is 15%, recorded as N-4; the volume percentage of microbial-based composite nano oil-displacing agent is 10%, recorded as N-3; the volume percentage of microbial-based composite nano oil-displacing agent is 5%, recorded as N-2; formation water is used as the control group, recorded as N-1. The formation water used is simulated formation water with a mineralization of 10,000, and the specific formula is (g / L): Na2SO40.0665, NaCl 8.893, CaCl20.571, MgCl20.432, NaHCO30.276.
[0134] The surface tension data of the microbial nano-oil-displacing agent treated above were measured using a surface tension meter.
[0135] Use the outer flame of an alcohol lamp to burn the platinum sheet to red, cool it to room temperature, adjust the tension meter to zero, and use deionized water to adjust the surface tension meter to zero to 72mN / m. Let the platinum sheet slowly contact the surface of the liquid to be tested. The surface tension of the liquid will pull the platinum sheet down. When the test value is stable, record the surface tension of the sample. The measured surface tension data is shown in Table 4.
[0136] Table 4 Surface tension results of microbial-based composite nano oil-displacing agent prepared in Example 10 at different concentrations
[0137] Serial number Microbial-based composite nano-oil displacement agent concentration Surface tension value (mN / m) N-1 Formation water 72.0 N-2 5% 42.5 N-3 10% 41.7 N-4 15% 39.6 N-5 20% 37.1 N-6 25% 36.2 N-7 30% 34.5 N-8 35% 33.7 N-9 40% 32.1 N-10 45% 31.6 N-11 50% 30.5 N-12 100% 25.8
[0138] According to the data in Table 4, as the concentration of microbial-based composite nano-oil-displacing agent increases, the surface tension continues to decrease, and the lowest can reach 25.8 mN / m. It can be proved that microbial-based composite nano-oil-displacing agent can also reduce the surface tension to a lower level.
[0139] Embodiment 18
[0140] The microbial-based composite nano oil-displacing agent stock solution prepared in Example 10 was diluted in a certain proportion. The interfacial tension of crude oil-nano oil-displacing agent was measured using an interfacial tension meter based on the spinning drop method. The spinning drop method can more accurately measure the interfacial tension between the crude oil-nano fluid phase and the interfacial tension variation law. Under the action of centrifugal force, gravity and interfacial tension, the low-density phase crude oil forms a long spherical or cylindrical droplet in the high-density phase nanofluid. The drop length (L) and width (D) values of the droplet, the density difference (Δρ) of the two-phase liquid and the rotation speed can be measured to calculate the interfacial tension value. The basic experimental steps are as follows:
[0141] The density of the oil phase and nanofluid used in the experiment was measured and the density difference was calculated;
[0142] Turn on the interfacial tension meter and adjust the experimental temperature to the required temperature;
[0143] Rinse the sample tube with the test solution;
[0144] Use a microsyringe to slowly fill the sample tube with nanofluid, avoiding the generation of bubbles during the whole process;
[0145] Use another microsyringe to inject the oil sample into the sample tube so that it is in the middle of the sample tube. Be careful not to stick to the tube wall. Then cover the sample tube cap to avoid bubbles in the sample tube and the cap.
[0146] The required rotation speed of the experiment was set, and the length and width of the oil droplet were measured every 10 minutes. The interfacial tension was calculated using the formula given by the instrument. After three measurements without change, the interfacial tension of the nanomaterials at different concentrations can be obtained, as shown in Table 5.
[0147] Table 5 Interfacial tension results of microbial-based composite nano oil-displacing agent prepared in Example 10 at different concentrations
[0148]
[0149] It can be seen from Table 5 that with the increase of the concentration of microbial-based composite nano-oil-displacing agent in the sample, the interfacial tension first decreases rapidly and then tends to be stable. The average interfacial tension is 0.05912 mN / m at the lowest and 0.34431 mN / m at the highest.
[0150] Embodiment 19
[0151] In order to verify the ability of microbial-based composite nano-oil-displacing agents to change the wettability of reservoir rocks, the change amount and change law of the contact angle were measured and recorded in the oil-water-solid three-phase system. The liquid phases were simulated formation water and microbial-based composite nano-oil-displacing agents of different concentrations, and the oil phase was simulated crude oil. The specific experimental steps are as follows:
[0152] The quartz glass sheet was pre-treated by soaking it in crude oil and aging it in an oven at 60°C for more than one week, and then taken out for use;
[0153] In a fume hood, clean the glass slide with n-heptane until the surface turns slightly yellow or colorless, and then wait for the n-heptane on the surface of the glass slide to evaporate;
[0154] 2 to 3 h before the experiment, the glass slide was immersed in different concentrations of microbial-based composite nano-oil-displacing agent. The concentrations of different concentrations of microbial-based composite nano-oil-displacing agent are shown in Table 6. The microbial-based composite nano-oil-displacing agent was allowed to change the wettability of the glass slide.
[0155] The hanging drop method was used to study the degree of contact angle change. The treated glass slide was placed in the sample tank, and the microbial-based composite nano-oil-displacing agent was added to cover the glass slide.
[0156] Start the image measurement and analysis equipment, adjust the position of the sample slot according to the image presented on the display screen, and ensure that the experimental sample can be clearly displayed and recorded on the display;
[0157] Use a curved needle to slowly drip simulated crude oil onto the lower surface of the glass slide in the sample pool. After the oil drop is stable, take a photo and record it, and get the contact angle value on the software.
[0158] Corresponding relationship and contact angle test results of the unprepared nano-samples of the same concentration in Example 10 Figure 11 to Figure 14 shown.
[0159] Table 6 Contact angle measurement samples of different concentrations of microbial-based composite nano oil-displacing agent prepared in Example 10
[0160] Serial number Microbial-based composite nano-oil displacement agent concentration J-1 Formation water J-2 5% J-3 10% J-4 20% J-5 30% J-6 40% J-7 50% J-8 100%
[0161] At 60℃, the contact angles of crude oil-simulated formation water and crude oil-microorganism-based composite nano-oil-displacing agent at different concentrations were measured. Figure 11 to Figure 14 It can be seen that the contact angle measured in the simulated formation water is 152.6°. After adding the microbial-based composite nano-oil-displacing agent, the contact angle measured is much smaller than that of the blank group, with the minimum being 30°, indicating that the microbial-based composite nano-oil-displacing agent has a significant effect on improving the wettability of reservoir rocks.
[0162] Embodiment 20
[0163] The glass micromodel used has a size of 5 cm × 5 cm and a permeability of 1 μm. 2, pore diameter is 20-100μm, porosity is 32.34%, wettability is water-wet, and the microbial-based composite nano oil-displacing agent synthesized in Example 10 is selected. The crude oil used in the experiment is at 60°C and has a viscosity of 3.47mPa·s. The microscopic model oil displacement system usually includes a micro-injection pump, a glass micro-model plate, and a set of image recording and processing equipment. The type of residual oil after water flooding and the distribution of residual oil after flooding with a microbial-based composite nano oil-displacing agent are studied to clarify the oil displacement mechanism of bio-nanofluids from a microscopic perspective. The specific experimental steps are as follows:
[0164] To avoid clogging of the model by large particles in the crude oil, the experimental oil was first centrifuged at 10,000 rpm for 15 min, and the upper layer of oil was collected after filtering with filter paper;
[0165] The inlet of the glass micromodel was connected to the micropump with a customized pipeline, and the outlet was drained into a measuring cylinder with a pipeline, and real-time images of the displacement process were taken through a microscope;
[0166] The glass micro-model is evacuated and saturated with simulated formation water. Saturation is complete when there is continuous water flow at the outlet.
[0167] The simulated crude oil was injected at a constant rate of 0.05 mL / m until no water flowed out of the outlet, which was considered as crude oil saturation.
[0168] First, simulated formation water was injected at a rate of 0.05 mL / m for water flooding, and the water flooding was stopped when the water content at the outlet was ≥98%;
[0169] Inject the microbial-based composite nano-oil displacement agent at a rate of 0.05 mL / m, and stop when the water content at the outlet is ≥98%;
[0170] The distribution of oil and water in the model after water flooding and microbial-based composite nano-oil flooding agent flooding was observed and recorded using a microscope. Fig.15 shown.
[0171] like Fig.15 The experimental results of microscopic oil displacement with different displacement fluids are shown. By comparing the pictures, it can be seen that after the water flooding, a large amount of residual oil cannot be displaced in the model. On the basis of water flooding, most of the residual oil is displaced after the microbial-based composite nano-oil-displacing agent is displaced, indicating that the microbial-based composite nano-oil-displacing agent can penetrate into more complex and finer formation pores to play a role, and significantly improve the oil displacement effect.
[0172] Embodiment 21
[0173] A simulated core displacement experiment was conducted on the microbial-based composite nano oil-displacing agent synthesized in Example 10 to evaluate the oil displacement effects of oil-displacing agents of different concentrations and confirm their oil displacement capabilities. The specific experimental method is as follows:
[0174] The core used in the experiment is an artificial core with a core size of The oil used in the experiment has a viscosity of 3.47 mPa·s at 60°C. The formulation of the formation water with a salinity of 10,000 is (g / L): Na2SO4 0.0665, NaCl 8.893, CaCl2 0.571, MgCl2 0.432, NaHCO3 0.276.
[0175] a. Select multiple cores with similar specifications and different permeabilities, dry them at 100℃ to constant weight, weigh the dry weight and calculate the core volume.
[0176] b. Place the dried core into simulated formation water for saturation for more than 48 hours, take it out and wipe it dry, weigh its wet weight, and calculate the pore volume and porosity;
[0177] c. Place the core in the core holder, apply annular pressure, and evacuate for 4 hours. Open the oven, set the temperature to 60°C, saturate the core with simulated formation water, and make the ions in the simulated formation water evenly distributed in the core;
[0178] d. Oil saturation. Inject a certain volume of crude oil into the core at 0.5 mL / min to saturate the core with crude oil, turn off the horizontal flow pump, close the gate valve, and keep it at a constant temperature for more than 48 hours to simulate the aging of crude oil in the formation;
[0179] e. Water flooding. Inject simulated formation water of a certain concentration and volume at 0.5 mL / min, and perform water flooding on the core saturated with crude oil. When the water content of the driven fluid at the outlet reaches 98% and the pressure is basically stable, stop the water flooding and measure the content of the displaced crude oil;
[0180] h. Nano-drive. On the basis of the above steps, continue to inject the microbial-based composite nano-oil-displacing agent synthesized in Example 10 at 0.5 mL / min. When the water content of the driven liquid at the outlet reaches 98% and the pressure is basically stable, stop the nano-drive and measure the content of the displaced crude oil;
[0181] i. Repeat the above steps with different concentrations of bio-nano oil-displacing agents.
[0182] The core related parameters and experimental results are shown in Table 7.
[0183] Table 7 Results of core simulation oil displacement experiments with different permeabilities
[0184]
[0185] It can be seen from Table 7 that the recovery rate of the cores under different permeabilities is different for the microbial-based composite nano oil-displacing agent synthesized in Example 10. Under the condition of medium porosity, the bimetallic nano oil-displacing agent can increase the recovery by 9.2% in 8mD cores, 11.2% in 50mD cores, and 13.2% in 400mD cores, indicating that the nano oil-displacing agent has a good effect on increasing the production and recovery of crude oil.
[0186] In summary, the fermentation liquid of the Bacillus subtilis strain BC23 provided by the present invention can be used to prepare a microbial-based composite nano-oil-displacing agent, which can reduce the contact angle of the crude oil-nanofluid system and significantly improve the wettability of reservoir rocks; it can penetrate into more complex and finer formation pores to exert its effect, and significantly improve the oil recovery effect.
[0187] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A microbial-based composite nano oil-displacing agent, characterized in that: The composition comprises: bimetallic nanoparticles and fermented bacterial liquid; the bimetallic nanoparticles include nanosilver and nanozinc oxide; The average particle size of the bimetallic nanoparticles is 37 nm; The fermentation broth is a fermentation broth of Bacillus subtilis strain BC23; the deposit number of the strain BC23 is: CCTCC NO.M2023700; The preparation method of the microbial-based composite nano oil-displacing agent comprises the following steps: mixing the silver ion solution and the zinc ion solution to obtain a metal precursor solution; The metal precursor solution is mixed with the fermentation bacterial solution and then cultured to obtain a microbial-based composite nano oil-displacing agent; The molar concentration ratio of silver ions to zinc ions in the metal precursor solution is 0.25:0.75; The volume ratio of the metal precursor solution to the fermentation liquid is (1-3):(1-3); The culture temperature is 35°C to 37°C; The culture time is 12 to 48 hours.
2. The microbial-based composite nano oil-displacing agent according to claim 1, characterized in that: The fermentation broth includes emulsifier and surfactant components; the fermentation broth includes aromatic and aliphatic substances.
3. The microbial-based composite nano oil-displacing agent according to claim 1, characterized in that: The method for preparing the fermentation broth comprises the following steps: The Bacillus subtilis strain BC23 is cultured in a culture medium to obtain a fermentation solution.
4. The microbial-based composite nano oil-displacing agent according to claim 3, characterized in that: The culture medium is a fermentation medium; the composition of the fermentation medium includes the following raw materials in percentage by weight: C6H 12 O61.0%-1.5%, Na2SO40.2%-0.5%, K2HPO4·3H2O 0.2%-0.5%, NH4Cl 0.1%-0.2%, MgCl2·6H2O0.02%-0.06%, sodium lactate 0.2%-0.4%, and the balance is deionized water. The sum of the mass percentages of the above components is 100%. The pH of the fermentation medium is preferably 7.0-7.
5.
5. The microbial-based composite nano oil-displacing agent according to claim 4, characterized in that: The composition of the fermentation medium includes the following raw materials in percentage by weight: C6H 12 O61.0%, Na2SO40.2%, K2HPO4·3H2O 0.2%, NH4Cl0.1%, MgCl2·6H2O 0.03%, sodium lactate 0.2%, and the balance is deionized water. The sum of the mass percentages of the above components is 100%.
6. The microbial-based composite nano oil-displacing agent according to claim 3, characterized in that: The culture temperature is 35° C. to 37° C.; the culture time is 3 to 7 days; and the culture rotation speed is 150 to 300 rpm.
7. The method for preparing the microbial-based composite nano oil-displacing agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: mixing the silver ion solution and the zinc ion solution to obtain a metal precursor solution; The metal precursor solution is mixed with the fermentation bacterial solution and then cultured to obtain a microbial-based composite nano oil-displacing agent; The molar concentration ratio of silver ions to zinc ions in the metal precursor solution is 0.25:0.75; The volume ratio of the metal precursor solution to the fermentation liquid is (1-3):(1-3); The culture temperature is 35°C to 37°C; The culture time is 12 to 48 hours.
8. The preparation method according to claim 7, characterized in that: The zinc ion solution includes zinc acetate hexahydrate solution; the silver ion solution includes silver nitrate solution.
9. The preparation method according to claim 7, characterized in that: The culture time is 24 hours.
10. Use of the microbial-based composite nano oil-displacing agent according to any one of claims 1 to 6 or the microbial-based composite nano oil-displacing agent prepared by the preparation method according to claim 7 or 8 in oil field production and / or improving crude oil recovery.
Citation Information
Patent Citations
Lipopetide biosurfactant oil extraction agent for improving extraction rate of crude oil
CN102504789A
Ag / Fe3O4 nano composite material and preparation method thereof
CN117106427A