A flexible substrate material and preparation method thereof

By introducing hydrogen bonds and inorganic nanofillers into the silicone resin material, forming dynamic bonds and synergistic effects, the shortcomings of polymer materials in mechanical and high-temperature resistance are solved, and a flexible substrate material with high toughness and high-temperature resistance are achieved. in electronic equipment.

CN117924613BActive Publication Date: 2024-11-22HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311718055.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-11-22
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

It is difficult for ordinary polymer materials to meet the requirements in terms of mechanical properties, elongation of break, tensile strength and high temperature resistance, which limits their application in the field of electronic materials.

Method used

An organic silicone resin material containing hydrogen bonds is used, and inorganic nanofillers are added to its matrix. The synergistic effect of dynamic bonds and inorganic nanofillers is formed through specific preparation methods to improve the mechanical properties of the material.

Benefits of technology

The material has excellent toughness, super tensile properties and high thermal decomposition temperature, with an elongation of break of 3120%, a tensile strength of 2.4MPa, a toughness of 41.68MJ/m3, and a 5% thermal weight loss temperature of 466℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117924613B_ABST
    Figure CN117924613B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and relates to a flexible substrate material and a preparation method thereof. The flexible substrate material is prepared from silicone resin, initiator, chain extender, amino reagent, catalyst and inorganic nanofiller under high temperature hot pressing conditions, and the preparation process mainly includes: (1) synthesis of silicone resin; (2) synthesis of organic silicone resin containing hydrogen bonds; (3) preparation of inorganic nanofiller flexible substrate material. The substrate material prepared in this way contains hydrogen bonds between molecules, has excellent stretchability and high temperature resistance, and its elongation at break can reach 3120%, and its 5% thermal weight loss temperature can reach 466°C. The preparation method is simple and has broad application prospects in the field of flexible electronic materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flexible stretchable polymer materials, and in particular relates to a flexible substrate material and a preparation method thereof. Background Art

[0002] As flexible electronic devices are gaining momentum, stretchable screens have become the next target in the display field. In addition to requiring improvements to existing designs and manufacturing processes, the realization of flexible display technology also puts forward new requirements for the performance of materials during processing and use. The development of substrate materials with excellent comprehensive performance has become a key link in realizing flexible displays. At present, materials that can be used as flexible display substrates include polymer substrates, ultra-thin glass substrates, stainless steel substrates, paper substrates, and biocomposite film substrates. Polymer materials have the advantage of strong chemical structure design. Through reasonable molecular design, a wide variety of polymer substrate materials can be obtained to meet the needs of different application fields.

[0003] However, it is difficult for ordinary polymer materials to simultaneously meet the requirements of mechanical properties such as material toughness, elongation at break, tensile strength and high temperature resistance, which limits their application in the field of electronic materials. There are many types of silicone polymers, such as liquid type and compound type. The usual method of modifying silicone polymers is to dissolve the matrix in an organic reagent for reaction, which may affect the mechanical properties of the product; the mechanical properties of the polymer can be enhanced by cross-linking, but excessive cross-linking often makes the material brittle and reduces elasticity; adding fillers and physically compounding with the matrix will cause too many defects in the matrix and be detrimental to the mechanical properties of the material. Summary of the invention

[0004] In response to the above problems, the purpose of the present invention is to provide a flexible substrate material, which contains hydrogen bonds between molecular chains and inorganic nanofillers, thereby effectively ensuring the excellent toughness of a flexible and stretchable silicone resin-based composite material. The silicone resin material also has a high thermal decomposition temperature, excellent tensile properties and high temperature resistance.

[0005] To achieve the above object, the present invention adopts the following technical solution: a flexible substrate material,

[0006] The molecular chain of the elastomer contains structure 1, and hydrogen bond structure 2 can be formed between molecules;

[0007]

[0008] A second object of the present invention is to provide a method for preparing the above-mentioned flexible substrate material, comprising the following steps:

[0009] 1) taking 30 parts by mass of silicone rubber, the side chains of which contain methyl and vinyl groups, and melting and stirring the silicone rubber at 100-120° C. for 2-10 minutes to obtain a rubber slurry;

[0010] 2) adding 0.02-0.15 parts by weight of an initiator to the rubber slurry and stirring evenly, then sequentially adding 0.01-0.1 parts by weight of a catalyst, 0.1-0.5 parts by weight of a chain extender, and 0.1-0.5 parts by weight of an amino reagent, stirring for 1-2 hours, and then adding 2-10 parts by weight of an inorganic nanofiller and stirring for 10-20 minutes to obtain a mixed slurry;

[0011] 3) The mixed slurry is allowed to stand for 12-36 hours, and then pressed into sheets at 140-170° C. and 2-10 MPa pressure. After solidification, the mixed slurry is placed at 180-220° C. for 2-6 hours to obtain a flexible substrate material.

[0012] Further improvement of the preparation method of flexible substrate materials:

[0013] Preferably, the molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:1.

[0014] Preferably, the silicone rubber is one or a combination of two or more of 107 silicone rubber, methyl vinyl silicone rubber and phenyl vinyl silicone rubber.

[0015] Preferably, the chain extender is one or a combination of two or more of isocyanoethyl methacrylate, cyclohexyl isocyanate, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, 2-isocyanoethyl acrylate, 4-acetoxystyrene, allyl isocyanate, diallyl isocyanurate, triallyl isocyanurate and tris(2-acryloyloxyethyl) isocyanurate.

[0016] Preferably, the amino reagent is one or a combination of two or more of 2-amino-4-hydroxy-6-methylpyrimidine, 2-vinyl-4,6-diamino-1,3,5-triazine, 3-vinylaniline, 4-vinylbenzylamine, 3-(hydroxyamino)-3-iminopropionic acid ethyl ester, 3-(2-aminoethoxy)propionic acid tert-butyl ester, 3-[2-(2-aminoethoxy)ethoxy]propionic acid tert-butyl ester, 4-amino-6-hydroxypyrimidine, 2-amino-4,6-dihydroxypyrimidine, N-(2-hydroxyethyl)ethylenediamine, (2-hydroxyethyl)hydrazine, 1,1-diethylurea and β-hydroxyethylurea.

[0017] Preferably, the catalyst is one or a combination of two or more of dibutyltin oxide, dibutyltin dibutyrate, dioctyltin dibutyrate, dibutyltin dilaurate, dimethyltin diacetate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, triethanolamine, N,N-dimethylbenzylamine and N,N'-lutidine.

[0018] Preferably, the initiator is one or a combination of two or more of dibenzoyl peroxide, tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, tert-butyl perbenzoate, cyclohexanone peroxide, di-tert-butyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0019] Preferably, the inorganic nanofiller is one or a combination of two or more of aluminum oxide, iron oxide, carbon nanotubes, graphene, carbon fiber, and zinc oxide.

[0020] Preferably, in step 3), a flat plate vulcanizing machine is used for tableting.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The present invention provides a flexible substrate material. Thanks to hydrogen bonding and relying on the synergistic effect of inorganic nanoparticles, the hydrogen-bonded flexible substrate material of the present invention exhibits excellent temperature resistance and super tensile properties. The nanoparticles play a reinforcing role and improve the mechanical properties of the material. In addition, the synergistic effect of the inorganic nanofiller and the polymer matrix also greatly improves the elongation at break of the material.

[0023] Thanks to the combined effect of dynamic bonds and inorganic nanofillers, the elongation at break of the hydrogen-bonded flexible substrate material of the present invention can reach 3120%, the tensile strength can reach 2.4 MPa, and the toughness can reach 41.68 MJ / m 3 , 5% thermal weight loss temperature reaches 466℃.

[0024] 2) The present invention provides a method for preparing a flexible substrate material. The preparation process and product structure of the hydrogen-bond-containing silicone resin are as follows:

[0025]

[0026] Silicone rubber has reactive methyl and vinyl groups, which can react with each other to form macromolecular chains through free radical polymerization, or react with small molecules containing double bonds to modify the matrix. There are hydrogen bonds between the chains of the material prepared by the present invention. This dynamic non-covalent bond plays a great role in the interaction force between the molecular chains of the material, and can be broken and reorganized under external forces. For example, under a certain rate of stretching, reversible dynamic bonds such as hydrogen bonds in the material can dissipate energy, so that the elongation at break of the material is improved, and the material exhibits better toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The stress-strain curves of the silicone-based elastomer material prepared in the comparative example and the flexible substrate material prepared in Examples 1 and 2;

[0028] Figure 2 The thermogravimetric curves of the silicone-based elastomer material prepared in the comparative example and the flexible substrate materials prepared in Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0030] Comparative Example

[0031] This comparative example provides a method for preparing a silicone resin-based elastomer material, using the following raw materials:

[0032] Silicone rubber: methyl vinyl silicone rubber (molecular weight about 600000);

[0033] Initiator: 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (C 16 H 34 O4), referred to as DBPH.

[0034] The specific preparation method comprises the following steps:

[0035] 1) Add 30g of methyl vinyl silicone rubber to the torque rheometer and stir at 120°C for 5 minutes. The side chain of methyl vinyl silicone rubber contains methyl and vinyl groups, and its structural formula is as follows:

[0036]

[0037] 2) Add 0.02 g of DBPH as an initiator and continue stirring for 5 minutes. The structural formula of the initiator DBPH is as follows:

[0038]

[0039] 3) Take out the sample and place it for 24 hours, then react it on a flat vulcanizer at 2-10MPa and 170℃ for 15 minutes. The vinyl groups in the side chains of the silicone rubber molecular chains undergo addition reaction, connecting the silicone rubber molecules to form a three-dimensional network structure. Then place the sample at 200℃ for 4 hours to obtain a silicone resin-based elastomer material. The reaction equation is as follows:

[0040]

[0041] Example 1

[0042] This embodiment provides a method for preparing a flexible substrate material, using the following raw materials:

[0043] Silicone rubber: methyl vinyl silicone rubber (molecular weight about 600000);

[0044] Initiator: 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, referred to as DBPH;

[0045] Catalyst: dibutyltin dilaurate, referred to as DBTDL;

[0046] Chain extender: 2-isocyanatoethyl acrylate (C6H7NO3), referred to as ICA;

[0047] Amine reagent: 2-amino-4-hydroxy-6-methylpyrimidine (C5H7N3O), referred to as UPY;

[0048] The specific preparation method comprises the following steps:

[0049] 1) Take 30g of silicone rubber (methyl vinyl silicone rubber), add it into a torque rheometer at 120°C and melt and stir for 5 minutes to obtain rubber slurry;

[0050] 2) Add 0.02g of initiator DBPH to the rubber slurry and continue stirring for 5 minutes; then add 0.02g of catalyst DBTDL, 0.125g of chain extender ICA, and 0.148g of amino reagent UPY in sequence, stir and react for 1 hour to obtain a mixed slurry; the molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:1. The chain extender ICA contains both carbon-carbon double bonds and isocyanate groups, which react with the amino groups in UPY to generate intermediate A, the structural formula of which is shown below:

[0051]

[0052] 3) The mixed slurry is allowed to stand for 24 hours, and then placed on a 170°C flat vulcanizer, and pressed into a sheet at a pressure of 5MPa. After curing, it is placed at 200°C for 4 hours. The initiator initiates free radical polymerization, and the above-mentioned small molecule intermediate A reacts with the double bond in the methyl vinyl silicone rubber to obtain a flexible substrate material. The reaction equation is as follows:

[0053]

[0054] The material was cut into dumbbell shape (50 mm long and 4 mm wide) with a cutter, and the mechanical properties were tested using a universal tensile testing machine (Yangzhou Tianyou TY-5000) with a tensile rate of 20 mm / min to obtain the stress-strain curve of the material. The tensile toughness of the material can be obtained by calculating the area under the curve. Thermogravimetric analysis was performed on a TG 209F3 (Netzsch, Germany) thermogravimetric analyzer with a heating rate of 10°C / min and a temperature range of 50°C to 700°C to analyze the high temperature resistance of the material.

[0055] Example 2

[0056] This embodiment provides a method for preparing a flexible substrate material, using the following raw materials:

[0057] Silicone rubber: 107 silicone rubber;

[0058] Initiator: tert-butyl hydroperoxide;

[0059] Catalyst: dibutyltin dibutyrate;

[0060] Chain extender: cyclohexyl isocyanate;

[0061] Amine reagent: ethyl 3-(hydroxyamino)-3-iminopropionate;

[0062] Inorganic nanofiller: nano alumina.

[0063] The specific preparation method comprises the following steps:

[0064] 1) Take 30g of 107 silicone rubber, add it into a torque rheometer at 110°C and melt and stir for 5 minutes to obtain rubber slurry;

[0065] 2) Add 0.02g of initiator tert-butyl hydroperoxide to the rubber slurry and continue stirring for 5min; then add 0.02g of catalyst dibutyltin dibutyrate, 0.125g of chain extender cyclohexyl isocyanate, and 0.148g of amino reagent 3-(hydroxyamino)-3-iminopropionic acid ethyl ester in sequence, stir and react for 1h, then add 6 parts by mass of nano-alumina and stir for 20min to obtain a mixed slurry; the molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:1;

[0066] 3) The mixed slurry was allowed to stand for 24 hours, and then placed on a 170°C flat vulcanizer, pressed into sheets at a pressure of 5 MPa, and after solidification, placed at 200°C for 4 hours to obtain a flexible substrate material.

[0067] Example 3

[0068] This embodiment provides a method for preparing a flexible substrate material, using the following raw materials:

[0069] Silicone rubber: methyl vinyl silicone rubber (molecular weight about 600000);

[0070] Initiator: 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, referred to as DBPH;

[0071] Catalyst: dibutyltin dilaurate, referred to as DBTDL;

[0072] Chain extender: 2-isocyanatoethyl acrylate (C6H7NO3), referred to as ICA;

[0073] Amine reagent: 2-amino-4-hydroxy-6-methylpyrimidine (C5H7N3O), referred to as UPY;

[0074] Inorganic nanofillers: graphene.

[0075] The specific preparation method comprises the following steps:

[0076] 1) Take 30g of silicone rubber (methyl vinyl silicone rubber), add it into a torque rheometer at 120°C and melt and stir for 5 minutes to obtain rubber slurry;

[0077] 2) Add 0.02 g of initiator DBPH to the rubber slurry and continue stirring for 5 min; then add 0.02 g of catalyst DBTDL, 0.125 g of chain extender ICA, and 0.148 g of amino reagent UPY in sequence, stir and react for 1 h, then add 5 parts by mass of graphene and stir for 20 min to obtain a mixed slurry; the molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:1.

[0078] 3) The mixed slurry was allowed to stand for 24 hours, and then placed on a 170°C flat vulcanizer, pressed into sheets at a pressure of 5 MPa, and after solidification, placed at 200°C for 4 hours to obtain a flexible substrate material.

[0079] The silicone resin-based elastomer material obtained in the comparative example and the flexible substrate material obtained in Examples 1-3 were cut into dumbbell shapes (50 mm in length and 4 mm in width) with a cutter, and the mechanical properties were tested using a universal tensile testing machine (Yangzhou Tianyou TY-5000) at a tensile rate of 20 mm / min to obtain the stress-strain curve of the material, and the tensile toughness of the material was obtained by calculating the area under the curve. Thermogravimetric analysis was performed on a TG 209F3 (Netzsch, Germany) thermogravimetric analyzer at a heating rate of 10°C / min and a temperature range of 50°C to 700°C to analyze the high temperature resistance of the material.

[0080] like Figure 1 , which are stress-strain curves of the silicone-based elastomer material obtained in the comparative example and the flexible substrate material obtained in Examples 1 and 2; Figure 1 It can be seen that the silicone resin-based elastomer material prepared in the comparative example does not contain hydrogen bonds and inorganic nanofillers, has an elongation at break of 830%, a tensile strength of 0.33 MPa, and a toughness of 0.203 MJ / m 3 The mechanical properties are average. The flexible substrate material prepared in Example 1 does not contain inorganic nanofillers, has an elongation at break of 1847%, a tensile strength of 0.18 MPa, and a toughness of 0.194 MJ / m 3 The elongation at break of the flexible substrate material obtained in Example 2 is 3120%, the tensile strength is 2.4 MPa, and the toughness can reach 41.68 MJ / m 3 ; From the comparison between the comparative example and Examples 1 and 2, it can be seen that by selecting silicone rubber with methyl and vinyl side chains as the matrix and introducing hydrogen bonds and inorganic nanofillers, the toughness and elongation at break of silicone resin can be greatly improved, thereby meeting the needs of different electronic equipment materials.

[0081] Example 3 introduces inorganic nanofillers based on Example 1. After testing, the elongation at break of the obtained flexible substrate material is 3215%, the tensile strength is 2.6 MPa, and the toughness can reach 43.52 MJ / m 3 Compared with the flexible substrate material prepared in Example 1, its elongation at break, tensile strength and toughness are significantly improved.

[0082] like Figure 2 As shown, the thermogravimetric curves of the silicone-based elastomer material prepared in the comparative example and the flexible substrate material prepared in Examples 1 and 2 are shown; Figure 2It can be seen that the 5% thermal weight loss temperature of the silicone resin-based elastomer material prepared in the comparative example is 406°C, and the 5% thermal weight loss temperature of the hydrogen-bonded flexible substrate material prepared in Example 1 exceeds 454°C, which proves that it has good heat resistance and is beneficial to extending the service life of the material in a high temperature environment; the 5% thermal weight loss temperature of the hydrogen-bonded flexible substrate material in Example 2 exceeds 466°C, which proves that it has good heat resistance and is beneficial to extending the service life of the material in a high temperature environment.

[0083] Example 3 introduces inorganic nanofillers on the basis of Example 1. After testing, the 5% thermal weight loss temperature of the prepared flexible substrate material exceeds 470° C., and the heat resistance is improved.

[0084] Those skilled in the art should understand that the above are only some specific embodiments of the present invention, rather than all embodiments. It should be noted that for those of ordinary skill in the art, many modifications and improvements can be made, and all modifications or improvements that do not exceed the scope of protection of the present invention should be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a flexible substrate material, characterized in that: The steps include: 1) Take 30 parts by mass of silicone rubber, the side chain of which contains methyl and vinyl groups, melt and stir the silicone rubber at 100-120° C. for 2-10 minutes to obtain a rubber slurry; the silicone rubber is methyl vinyl silicone rubber; 2) Add 0.02-0.15 parts by weight of initiator to the rubber slurry and stir evenly, then add 0.01-0.1 parts by weight of catalyst, 0.1-0.5 parts by weight of chain extender, and 0.1-0.5 parts by weight of amino reagent in sequence, stir to react for 1-2 hours, then add 2-10 parts by weight of inorganic nanofiller and stir for 10-20 minutes to obtain a mixed slurry; the chain extender is 2-isocyanatoethyl acrylate, and the amino reagent is 2-amino-4-hydroxy-6-methylpyrimidine; 3) The mixed slurry is allowed to stand for 12-36 hours, and then pressed into sheets at 140-170°C and 2-10 MPa pressure. After solidification, it is placed at 180-220°C for 2-6 hours to obtain a flexible substrate material.

2. The method for preparing a flexible substrate material according to claim 1, characterized in that: The molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:

1.

3. The method for preparing a flexible substrate material according to claim 1, characterized in that: The catalyst is one or a combination of two or more of dibutyltin oxide, dibutyltin dibutyrate, dioctyltin dibutyrate, dibutyltin dilaurate, dimethyltin diacetate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, triethanolamine, N,N-dimethylbenzylamine and N,N'-dimethylpyridine.

4. The method for preparing a flexible substrate material according to claim 1, characterized in that: The initiator is one or a combination of two or more of dibenzoyl peroxide, tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, tert-butyl perbenzoate, cyclohexanone peroxide, di-tert-butyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

5. The method for preparing a flexible substrate material according to claim 1, characterized in that: The inorganic nanofiller is one or a combination of two or more of aluminum oxide, iron oxide, carbon nanotubes, graphene, carbon fiber, and zinc oxide.

6. The method for preparing a flexible substrate material according to claim 1, characterized in that: In step 3), a flat plate vulcanizing machine is used for tableting.

7. A method for preparing a flexible substrate material, characterized in that: The steps include: 11) Take 30g of 107 silicone rubber, add it into a torque rheometer at 110℃ and melt and stir for 5 minutes to obtain rubber slurry; 12) Add 0.02g of initiator tert-butyl hydroperoxide to the rubber slurry and continue stirring for 5min; then add 0.02g of catalyst dibutyltin dibutyrate, 0.125g of chain extender cyclohexyl isocyanate, and 0.148g of amino reagent 3-(hydroxyamino)-3-iminopropionic acid ethyl ester in sequence, stir and react for 1h, then add 6 parts by mass of nano-alumina and stir for 20min to obtain a mixed slurry; the molar ratio of -NCO in the chain extender to the amino group in the amino reagent is 1:1; 13) The mixed slurry was allowed to stand for 24 hours, then placed on a 170°C flat vulcanizer, pressed into sheets at a pressure of 5 MPa, and after solidification, placed at 200°C for 4 hours to obtain a flexible substrate material.

8. A flexible substrate material obtained by the method for preparing a flexible substrate material according to any one of claims 1 to 7.