A microalgae-based composite hydrogel and preparation method thereof

By mixing gellan gum with the rheology regulator of microalgae and standing, forming a microalgae-based composite hydrogel with thermal stability and anti-freeze properties, the microalgae-based composite hydrogel in the composite gel in the prior art is solved. The problem that application potential has not been tapped has realized the application potential in multiple fields.

CN117924748BActive Publication Date: 2024-11-26LIAOCHENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410127234.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-11-26
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

The research on composite gelling and microalgae in the prior art is relatively limited, especially the diversity of active substances and rheology regulation of Viagra has not been fully explored, resulting in the potential value of its colloidal properties being unable to be effectively utilized.

Method used

By mixing the gellan gel dispersion with the rheology regulator dispersion, adding NaOH and CaCl2 solutions, it is left to stand to form a microalgae-based composite hydrogel, and using proteins, polysaccharides and other substances in the microalgae to produce gellan gelatin Physiological interactions change the rheological properties of the gel and release large particulate matter through treatment methods to enhance the stability and filling of the gel.

Benefits of technology

The prepared microalgae-based composite hydrogel has good thermal stability and anti-freeze properties, and has controllable rheological characteristics. It is suitable for special medical uses, formula food and biological medicine preparation fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117924748B_ABST
    Figure CN117924748B_ABST
Patent Text Reader

Abstract

The present invention discloses a microalgae-based composite hydrogel and a preparation method thereof, which belongs to the field of biomedical technology. A gellan gum dispersion and a rheology modifier dispersion are mixed to obtain a mixed dispersion, and a NaOH solution and a CaCl2 solution are sequentially added to the mixed dispersion, mixed, and allowed to stand to obtain the microalgae-based composite hydrogel, wherein the rheology modifier dispersion is prepared from microalgae powder. The present invention utilizes one or more methods of high-speed shearing, high-pressure homogenization, and ultrasound to process microalgae, effectively reducing the particle size of microalgae, utilizing Haematococcus pluvialis as a rheology modifier, modifying pure gellan gum hydrogel, and conducting relevant rheology studies on the obtained hydrogel. The properties of the composite hydrogel are controlled by processing the rheology modifier and controlling the amount of addition, so as to achieve application in multiple fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biomedicine technology, and in particular relates to a microalgae-based composite hydrogel and a preparation method thereof. Background Art

[0002] A general bio-based hydrogel is a complex three-dimensional structure composed of biopolymers, which is extensively cross-linked by physical and / or chemical means and exhibits hydrophilic or hydrophobic properties. Natural polymer-based composite hydrogels are made of a variety of materials and are low-cost. They have successfully entered the professional medical food industry and the general consumer market, launching many innovative products.

[0003] As an important component of natural polymers, polysaccharides have attracted extensive attention due to their bioactivity, inherent biodegradability and biocompatibility. These properties make polysaccharide materials highly sought after in food research, drug delivery, tissue engineering and wastewater treatment equipment development. Polysaccharides have excellent gelling, emulsifying and foaming properties, thereby enhancing the texture and flavor of food. Many microalgae have high protein content and high nutritional value. In recent years, there has been a strong interest in adding various microalgae as new protein sources to artificial gels.

[0004] However, research on composite gels based on gellan gum and microalgae is very limited, especially the diverse active ingredients and unique rheological regulation effects of microalgae, and exploring its colloidal properties has great potential value. Summary of the invention

[0005] The purpose of the present invention is to provide a microalgae-based composite hydrogel and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0006] One of the technical solutions provided by the present invention:

[0007] A method for preparing a microalgae-based composite hydrogel comprises the following steps: mixing a gellan gum dispersion and a rheology regulator dispersion to obtain a mixed dispersion, sequentially adding a NaOH solution and a CaCl2 solution to the mixed dispersion, mixing well, and standing to obtain the microalgae-based composite hydrogel, wherein the rheology regulator dispersion is prepared from microalgae powder.

[0008] The specific role of microalgae in composite hydrogels is that microalgae contain a variety of contents, such as proteins, polysaccharides, lipids, etc. By destroying microalgae through some treatment methods, not only these substances are released, but also some large particles are obtained with the destruction of cell walls, cell membranes and other structures. Proteins, polysaccharides and other substances have a variety of functional groups, which can produce physical interactions with gellan gum, thereby changing the rheological properties of the gel. At the same time, some large particles produced can fill the gel and stabilize the gel structure. Haematococcus pluvialis is rich in astaxanthin. By adding Haematococcus pluvialis to the hydrogel, the hydrogel can also carry astaxanthin to achieve the application of special medical food.

[0009] Preferably, the volume ratio of the rheology modifier dispersion to the gellan gum dispersion is (0.1-2):(5-10), and more preferably, the volume ratio of the rheology modifier dispersion to the gellan gum dispersion is 1:10.

[0010] Preferably, the volume ratio of the mixed dispersion, NaOH solution and CaCl2 solution is 11:1:2; more preferably, the molar concentration of the NaOH solution is 0.125mM-0.25M, and the molar concentration of the CaCl2 solution is 1mM-100mM.

[0011] In the present invention, NaOH solution and CaCl2 solution are used as crosslinking agents to make the gellan gel through ionic crosslinking. The reason why NaOH solution needs to be added first and then CaCl2 solution is that the NaOH solution added first can provide a suitable crosslinking environment, and then CaCl2 is added to complete the crosslinking.

[0012] Preferably, the standing temperature is 4-25°C and the time is 1-12 hours.

[0013] The role of standing: The cross-linking reaction occurs quickly, but after local cross-linking occurs, the cross-linking agent needs a certain amount of time to diffuse completely. By limiting the standing temperature, it is helpful to accelerate molecular movement and promote cross-linking. When 25°C is selected, molecular movement can be accelerated. In order to reduce the harm of microorganisms to the gel, 4°C can be selected.

[0014] Preferably, the preparation method of the rheology modifier dispersion is: adding microalgae powder to deionized water, stirring at room temperature to obtain a microalgae suspension, bathing the microalgae suspension, cooling to room temperature, and then shearing and ultrasonicating to prepare the rheology modifier dispersion.

[0015] The soluble protein and polysaccharide in the microalgae can be fully dissolved in the dispersion through the preparation method.

[0016] More preferably, the microalgae powder is selected from Haematococcus pluvialis powder, Dunaliella salina powder or Chlorella pyrenoidosa powder.

[0017] Preferably, the mass ratio of the microalgae powder to deionized water is (0.1-20):100, and more preferably, the mass ratio of the microalgae powder to deionized water is (2-10):100.

[0018] More preferably, the temperature of the water bath is 95° C. and the time is 15 min.

[0019] Preferably, the mass concentration of the gellan gum dispersion is 1-5%, and more preferably, the mass concentration of the gellan gum dispersion is 1%.

[0020] Preferably, the preparation method of the gellan gum dispersion is: take 0.1-10g gellan gum and add 100mL deionized water, and stir continuously for 3-5h at 10-50°C until a uniform dispersion is formed and dissolved. The more preferred stirring temperature is room temperature.

[0021] The second technical solution provided by the present invention is:

[0022] A microalgae-based composite hydrogel prepared by the preparation method.

[0023] Beneficial effects of the present invention:

[0024] The microalgae-based composite hydrogel provided by the present invention has good thermal stability, multiple controllable rheological properties, and certain anti-freezing performance.

[0025] The present invention uses one or more methods of high-speed shearing, high-pressure homogenization and ultrasound to process microalgae, effectively reducing the particle size of microalgae, destroying the structure of microalgae, releasing soluble protein and polysaccharide, using Haematococcus pluvialis as a rheology regulator, modifying pure gellan gum hydrogel, and conducting relevant rheology research on the obtained hydrogel. By processing the rheology regulator and controlling the addition amount, the properties of the composite hydrogel are controlled, so as to achieve application in multiple fields.

[0026] The present invention adds a specially treated rheology regulator to gellan gum to prepare a composite hydrogel with controllable rheological properties, certain thermal stability and anti-freezing performance, and predictable flow behavior and stiffness. The prepared composite hydrogel can be applied to special medical purposes, formulated foods and the field of biopharmaceutical preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0028] Figure 1 Thermogravimetric analysis (TGA) test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0029] Figure 2 The differential scanning calorimetry (DSC) test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0030] Figure 3 The rheological flow behavior test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0031] Figure 4 The rheological amplitude scanning test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0032] Figure 5 The rheological frequency scanning test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0033] Figure 6 The rheological dynamic temperature scanning test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0034] Figure 7 Creep test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2;

[0035] Figure 8 The rheological cycle time strain sweep test results of the composite hydrogels prepared in Examples 1-5 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0041] The embodiment of the present invention selects and processes a rheology modifier to obtain a rheology modifier dispersion; dissolves gellan gum to obtain a gellan gum dispersion; prepares a crosslinking agent to obtain a crosslinking agent solution; mixes the rheology modifier dispersion and the gellan gum dispersion, stirs them evenly, and obtains a mixed dispersion; adds the crosslinking agent solution to the mixed dispersion, stirs them evenly, and places them at 4 to 25° C. for 1 to 12 hours to prepare a composite hydrogel.

[0042] The room temperature in the present invention refers to 25±2°C.

[0043] The “parts” in the examples of the present invention all represent parts by mass.

[0044] The microalgae in the present invention can be selected from any one of Haematococcus pluvialis, Dunaliella salina and Chlorella pyrenoidosa. The following examples are conducted using Haematococcus pluvialis powder.

[0045] All raw materials in the examples of the present invention were purchased.

[0046] Example 1

[0047] A method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0048] S1. 2 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000rpm, shearing for 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shearing liquid, and the shearing liquid was ultrasonically treated (power 300w, ultrasonic switch time 3s each, total time 20min), and the obtained ultrasonic liquid was a rheology modifier dispersion;

[0049] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0050] S3. The rheology modifier dispersion and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0051] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHB.

[0052] Example 2

[0053] A method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0054] S1. 4 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000rpm, shearing for 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shearing liquid, and the shearing liquid was ultrasonically treated (power 300w, ultrasonic switch time 3s each, total time 20min), and the obtained ultrasonic liquid was a rheology modifier dispersion;

[0055] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0056] S3. The rheology modifier dispersion and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0057] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHC.

[0058] Example 3

[0059] A method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0060] S1. 6 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000rpm, shearing for 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shearing liquid, and the shearing liquid was ultrasonically treated (power 300w, ultrasonic switch time 3s each, total time 20min), and the obtained ultrasonic liquid was a rheology modifier dispersion;

[0061] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0062] S3. The rheology modifier dispersion and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0063] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHD.

[0064] Example 4

[0065] A method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0066] S1. 8 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000rpm, shearing for 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shearing liquid, and the shearing liquid was ultrasonically treated (power 300w, ultrasonic switch time 3s each, total time 20min), and the obtained ultrasonic liquid was a rheology modifier dispersion;

[0067] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0068] S3. The rheology modifier dispersion and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0069] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHE.

[0070] Example 5

[0071] A method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0072] S1. 10 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000rpm, shearing for 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shearing liquid, and the shearing liquid was ultrasonically treated (power 300w, ultrasonic switch time 3s each, total time 20min), and the obtained ultrasonic liquid was a rheology modifier dispersion;

[0073] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0074] S3. The rheology modifier dispersion and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0075] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHF.

[0076] Example 6

[0077] The same as Example 1, except that 0.1 parts of Haematococcus pluvialis powder is added in step S1.

[0078] Example 7

[0079] The same as Example 1, except that 20 parts of Haematococcus pluvialis powder are added in step S1.

[0080] Example 8

[0081] The same as Example 1, except that step S2 is to mix 5 parts of gellan gum and 100 parts of deionized water, and stir at room temperature for 3 hours to obtain a gellan gum dispersion.

[0082] Example 9

[0083] The same as Example 1, except that, in step S3, the rheology modifier dispersion and the gellan gum dispersion are mixed at a volume ratio of 0.1:10, and stirred for 3 minutes to obtain a mixed dispersion.

[0084] Example 10

[0085] The same as Example 1, except that, in step S3, the rheology modifier dispersion and the gellan gum dispersion are mixed at a volume ratio of 2:10 and stirred for 3 minutes to obtain a mixed dispersion.

[0086] Comparative Example 1

[0087] The same as Example 1, except that step S1 is not subjected to ultrasonic treatment.

[0088] Specifically, a method for preparing a microalgae-based composite hydrogel comprises the following steps:

[0089] S1. 2 parts of Haematococcus pluvialis powder and 100 parts of deionized water were mixed and stirred at room temperature for 12 hours to obtain a suspension of Haematococcus pluvialis after sufficient hydration. The obtained suspension of Haematococcus pluvialis was placed in a water bath (95°C, 15 minutes), then cooled to room temperature, and the cooled suspension was sheared at high speed (10000 rpm, 1 minute each time, repeated 5 times, each time with an interval of 1 minute) to obtain a shear liquid;

[0090] S2. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0091] S3. The shearing liquid and the gellan gum dispersion were mixed in a volume ratio of 1:10 and stirred for 3 min to obtain a mixed dispersion;

[0092] S4. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the mixed dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a microalgae-based composite hydrogel, namely GHG.

[0093] Comparative Example 2

[0094] S1. Mix 1 part of gellan gum and 100 parts of deionized water and stir at room temperature for 3h to obtain a gellan gum dispersion;

[0095] S2. NaOH solution (0.25 mM) and CaCl2 solution (10 mM) were sequentially added to the gellan gum dispersion, wherein the volume ratio of NaOH solution, CaCl2 solution and the mixed dispersion was 1:2:11. After stirring evenly, the mixture was allowed to stand at 4°C for 12 h to prepare a hydrogel, namely GHA.

[0096] Performance test

[0097] 1. Thermal stability test

[0098] Test method: The thermal stability of Examples 1-5 and Comparative Examples 1-2 was analyzed by thermogravimetric analysis (TGA). The freeze-dried composite hydrogel sample was placed in a platinum open pan, and the freeze-dried mass was controlled to be 0.5-5 mg. The temperature control program was set to heat from 25°C to 300°C at a heating rate of 10°C / min, and nitrogen was selected as the purge gas, and the purge rate was set to 50 mL / min.

[0099] The results of the test are as follows Figure 1 As shown: The thermal degradation curve of each sample shows that the degradation temperature of Examples 1-5 (GHB-GHF) and Comparative Example 1 (GHG) is between 235.3°C and 237.1°C. The degradation temperature of Comparative Example 2 (GHA) is 235.5°C. The thermal degradation peaks of each composite hydrogel (from GHB to GHG) are all single peaks, without secondary degradation peaks. It shows that the added Haematococcus pluvialis dispersion can form a uniform system with gellan gum without obvious phase separation. It can be seen from the data in Table 1 that the addition of Haematococcus pluvialis moderately reduces the hygroscopicity of the dry gel (composite hydrogel after freeze-drying), and the degradation temperature of each composite hydrogel is around 236°C.

[0100] Table 1

[0101]

[0102] 2. Freeze resistance test

[0103] Test method: Differential scanning calorimetry (DSC) was used to evaluate the antifreeze property. First, fresh hydrogel samples were weighed in an aluminum open pan. The mass of each sample was kept as consistent as possible (between 20-30 mg), and then the aluminum open pan was covered with an aluminum lid. The temperature control program was set to decrease from 20°C to -30°C at a constant temperature change rate of 10°C / min, and then increase from -30°C to 40°C. Nitrogen was used for blowing, and the blowing rate was set to 50 mL / min.

[0104] The results of the test are as follows Figure 2As shown: in the initial cooling process (from 20°C to -30°C), all composite hydrogels exhibited exothermic behavior; on the contrary, in the process of heating (-30 to 40°C), all composite hydrogels exhibited endothermic phenomena. The freezing points of all composite hydrogels are listed in Table 2. Compared with the hydrogel (GHA) of Comparative Example 2, the remaining composite gels exhibited higher freezing point temperatures. Among them, GHD had the highest freezing point temperature of -15.3°C, and the freezing points of other composite gel samples ranged from -16.3°C to -18°C. Overall, the freezing points of most composite hydrogels were below -16°C, showing excellent low-temperature protection properties. This property enables composite hydrogels to be used as carriers for preserving active substances (such as specific pharmaceutically active proteins) and for transporting nutrients that require low temperature conditions.

[0105] Table 2

[0106]

[0107] 3. Rheological flow behavior test

[0108] Test method: A rheometer was used to comprehensively evaluate the rheological properties of the composite hydrogel. The measurement system was a parallel plate measurement system, the upper plate was a stainless steel circular plate with a diameter of 50 mm, and the measurement gap between the upper plate and the lower plate was 1 mm. In order to evaluate the flow behavior of different composite hydrogel samples, the test temperature was set to 25 °C and the shear rate range was 0.01 to 100 s -1 Data collection is performed within.

[0109] The results are as follows Figure 3 As shown in the figure: The increase in shear rate leads to a gradual increase in the shear stress of GHA-GHG hydrogel. Figure 3 In (B), the yield stress of comparative example 2 (GHA) is 0.592Pa, and the yield stress of GHB~GHG is 0.81~2.617Pa. Compared with GHA, the yield stress values ​​of other composite hydrogels containing Haematococcus pluvialis increase. Obviously, the yield stress value is positively correlated with the concentration of Haematococcus pluvialis, which is consistent with the results observed in the actual experiment. At the same time, compared with GHB and GHG, the amount of Haematococcus pluvialis balls added is the same, but due to the larger particle size of the Haematococcus pluvialis balls in GHG, the yield stress value of GHG is significantly reduced. This feature can provide basic data for the development of edible gels with different textures and sensory qualities, and is convenient for customizing gel products according to the specific requirements of different customer groups.

[0110] 4. Rheological amplitude sweep test

[0111] Test method: The experimental temperature is controlled at 25°C, the amplitude scan is preferably controlled by strain, the strain scan frequency is 10Hz, and the dynamic scan strain is in a fixed range of 0.01% to 100%. Amplitude scanning can identify the linear viscoelastic region (LVR) and other related parameters, which helps to fully understand the various characteristics of hydrogels.

[0112] The results are as follows Figure 4 As shown in the figure, where G' represents the elastic modulus and G" represents the viscous modulus (for example, GHAG' represents the storage modulus of GHA and GHAG" represents the loss modulus of GHA), the elastic modulus of each composite hydrogel decreases when the LVR threshold is exceeded, indicating that yielding has occurred. The yield point is defined as the shear stress value at the LVR boundary. The yield stress of all composite hydrogel samples follows the following order: GHF (10 parts) > GHE (8 parts) > GHC (4 parts) > GHD (6 parts) > GHG (2 parts) > GHB (2 parts) > GHA. The results indicate that the addition of Haematococcus Pluvialis (HP) dispersion can improve the structural strength of pure gellan gum hydrogel. The yield stress ranking is highly consistent with the actual observation results. It is worth noting that GHF (10 parts) has the largest yield stress value among all composite hydrogels, indicating excellent mechanical strength compared with other composite hydrogels. The values ​​of GHC and GHD showed some fluctuations due to the combined effects of the particle size and concentration of the added Haematococcus pluvialis, and these changes originated from the fluctuating interaction between the particles and the gel matrix.

[0113] 5. Rheology frequency sweep test

[0114] Test method: The frequency sweep is intended to describe the time dependence of the sample within the non-destructive deformation range, with a strain of 0.1% and an angular frequency of 0.1 to 100 rad / s. Usually the frequency sweep is performed from high frequency to low frequency.

[0115] The results are shown in Figure 5, where G' represents the elastic modulus and G" represents the viscous modulus (e.g., GHAG' represents the storage modulus of GHA and GHAG" represents the loss modulus of GHA). In order to gain a deeper understanding of the viscoelastic properties exhibited by GHA-GHG, a comprehensive study involving frequency sweeps was conducted. This detailed analysis allowed the identification of the elastic modulus (G') and the viscous modulus (G"), as well as the tanδ value. Figure 5 As shown, the G' values ​​of all composite hydrogels exceeded their corresponding G" values, resulting in tanδ values ​​lower than 1, indicating that within the test frequency range, all composite hydrogels maintained ideal elastic conditions. By comparing the G' of the above composite hydrogels, it can be clearly seen that the addition of Haematococcus pluvialis dispersion can improve the stiffness of the composite hydrogel.

[0116] 6. Rheological temperature scanning test

[0117] Test method: To evaluate the heat resistance of the hydrogel, the test was carried out in the temperature range of 20°C to 80°C. In order to inhibit the evaporation of water, a narrow coating of silicone oil with a viscosity of 0.05 Pa was carefully applied along the edges of the parallel plates.

[0118] The results are as follows Figure 6 As shown in Figure 2, where G' represents the elastic modulus and G" represents the viscous modulus (e.g. GHA G' represents the storage modulus of GHA and GHA G" represents the loss modulus of GHA), temperature is of vital importance in different environments. During the production of composite hydrogels, heat occurs. This means that heat is generated when composite hydrogels are manufactured. This heat generation is an important factor to be considered in the entire manufacturing process. The regulation of temperature intricately changes the performance attributes of composite hydrogels, thereby affecting their application in daily and industrial environments.

[0119] from Figure 6 It can be clearly seen that the modulus of GHA-GHG changes significantly with increasing temperature. In the lower temperature range (T<55℃), the G' of all composite hydrogels exceeds G", showing typical solid-like behavior; as the temperature increases, the loss modulus of different composite hydrogels gradually exceeds the storage modulus, indicating that the composite hydrogel exhibits partial fluid-like behavior. The melting temperature (Tm) can be defined as the temperature at which G' and G" intersect during the temperature rise. Figure 6 As shown in the figure, the Tm order of all composite hydrogels is as follows: GHF (10 parts) > GHE > (8 parts) GHC (4 parts) > GHD (6 parts) > GHB (2 parts) > GHA > GHG (2 parts). The results show that the thermal stability of pure gellan gum hydrogel can be significantly enhanced by ultrasonic treatment of the sheared Haematococcus pluvialis dispersion and then mixing it with the gellan gum dispersion. Especially in the composite gel with a high concentration of Haematococcus pluvialis dispersion, the Tm of GHF reached 88.65℃, which is 47.5% higher than that of GHA (60.07℃). It is worth noting that the Tm of GHF is as high as 88.65℃, making it suitable for rapid high-temperature pasteurization. This advantage of high-temperature sterilization is crucial for industrial production and large-scale utilization of hydrogels in professional medical and food applications.

[0120] 7. Rheological creep test

[0121] Test method: Within 180s, all the above composite hydrogel samples underwent progressive stress application until reaching a maximum value of 0.5Pa, after which the pressure was rapidly released, and the resulting strain recovery was attributed to the internal structural reorganization of the hydrogel.

[0122] The results are as follows Figure 7As shown: Compared with GHB-GHG, GHA has the most significant strain, while GHE and GHF are hardly affected. In addition, the test curves also reveal that after removing the stress load, GHC, GHE, and GHF exhibit a relatively long recovery period before reaching the lowest plateau level. In contrast, GHA, GHB, GHD, and GHG show a rapid reach to the lowest plateau period. This indicates that GHC, GHE, and GHF exhibit partial viscous deformation, similar to the behavior observed in viscoelastic fluids. In contrast, samples such as GHA, GHB, GHD, and GHG show relatively rapid recovery, indicating less internal viscous deformation and retaining favorable elastic properties within the system.

[0123] 8. Rheological Thixotropy Test

[0124] Test method: To gain a deeper understanding of the self-recovery ability exhibited by the composite hydrogel, a series of cyclic time-strain scans were conducted. The composite hydrogel samples underwent changes from low strain to high strain, repeated 5 times, at a frequency of 10 Hz, with a low strain of 0.1% and a high strain of 200%.

[0125] The results are as Figure 8 shown, where G' represents the elastic modulus and G” represents the viscous modulus (for example, GHA G' represents the storage modulus of GHA, and GHA G” represents the loss modulus of GHA), and the different behaviors exhibited by each composite hydrogel sample under different strain conditions. Specifically, when subjected to small strains, all composite hydrogels exhibit a characteristic elastic state (G'>G”). In contrast, at large strains, most composite hydrogels (except GHG) maintain an obvious viscous state (G'<G”). After undergoing five consecutive cycles, due to the different internal structures of each hydrogel, there are quite significant differences in the degree of modulus recovery.

[0126] Among the composite hydrogels, the highest recovery rate of GHD is 70%, exceeding 64% of GHA. The recovery rates of the remaining composite hydrogels are between 46% and 69%. The results obtained confirm that although the above composite hydrogels all have the potential for partial structural recovery, they still experience some loss of integrity during external operations. Generally speaking, adding an appropriate concentration (such as GHD) of Haematococcus pluvialis dispersion can maintain or slightly enhance the self-recovery ability of the pure gellan gum hydrogel, while adding a high concentration (such as GHE and GHF) of Haematococcus pluvialis dispersion will reduce its recovery ability. This finding indicates that the recovery ability of the composite hydrogel can be regulated by controlling the addition amount of the Haematococcus pluvialis solution dispersion.

[0127] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a microalgae-based composite hydrogel, It is characterized in that The gellan gum dispersion and the rheology modifier dispersion were mixed to obtain a mixed dispersion, and NaOH solution and CaCl were added to the mixed dispersion in sequence. 2 solution, mixing and standing to obtain the microalgae-based composite hydrogel; the rheology modifier dispersion is prepared from microalgae powder; The preparation method of the rheology modifier dispersion is as follows: adding microalgae powder to deionized water, stirring at room temperature to obtain a microalgae suspension, bathing the microalgae suspension, cooling to room temperature, and then shearing and ultrasonicating to prepare the rheology modifier dispersion; The mass ratio of the microalgae powder to deionized water is (0.1-20):100; The temperature of the water bath is 95°C and the time is 15 minutes; The microalgae powder is Haematococcus pluvialis powder.

2. The preparation method according to claim 1, It is characterized in that The volume ratio of the rheology modifier dispersion to the gellan gum dispersion is (0.1-2): (5-10).

3. The preparation method according to claim 1, It is characterized in that The mixed dispersion, NaOH solution and CaCl 2 The volume ratio of the solution is 11:1:

2.

4. The preparation method according to claim 1, It is characterized in that The standing temperature is 4-25°C and the standing time is 1-12h.

5. The preparation method according to claim 1, It is characterized in that The mass concentration of the gellan gum dispersion is 1-5%.

6. A microalgae-based composite hydrogel prepared by the preparation method according to any one of claims 1 to 5.