High thermal conductivity filler for semiconductor flip chip packaging

Through the cross-linked network technology of vinyl-modified alumina, fullerene and other components, it solves the problem of difficult to balance thermal conductivity, hardness and elasticity in the existing technology, and realizes semiconductor flip-chip with high thermal conductivity and structural stability. Chip packaging materials improve the overall performance and durability of the package.

CN117925182BActive Publication Date: 2024-10-22NANJING JUDING CORE MATERIAL TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410133540.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-31
Publication Date
2024-10-22
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Existing semiconductor flip-chip packaging materials are difficult to satisfy thermal conductivity, hardness, elasticity and structural toughness at the same time, resulting in poor adhesion or the inability to form an effective inorganic stacking thermal conductive network.

Method used

Using components such as vinyl-modified alumina, fullerene, vinyl-terminated silicone oil, hydrogen-containing silicone oil and Pt catalyst, the vinyl silicone oil and hydrogen-containing silicone oil form a cross-linked network under the action of Pt catalyst, and utilize fullerene The cyclic vinyl group reacts with the active hydrogen of hydrogen-containing silicone oil to form an interpenetrating cross-linked network of inorganic particles and polymer chains, improving thermal conductivity and structural stability.

Benefits of technology

It achieves improvements in thermal conductivity, hardness, elasticity and mechanical strength, while ensuring the heat resistance, cold resistance and flame resistance of the filler, ensuring the durability and stability of the semiconductor package.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004690483370000091
    Figure BDA0004690483370000091
  • Figure BDA0004690483370000111
    Figure BDA0004690483370000111
Patent Text Reader

Abstract

The invention discloses a high thermal conductivity filling glue for semiconductor flip chip packaging, including vinyl modified alumina, fullerene, vinyl-terminated silicone oil, high vinyl silicone oil, hydrogen-containing silicone oil and Pt catalyst, and the surface of the fullerene is treated by cyclodextrin encapsulation. The invention forms a cross-linked network of inorganic particles and polymer chains interpenetrating each other by vinyl modification of the surface of alumina, and catalytic addition reaction of vinyl silicone oil and hydrogen-containing silicone oil under the action of Pt catalyst; utilizes the high reactivity of cyclovinyl groups rich in the surface of fullerene and the active hydrogen of hydrogen-containing silicone oil to serve as nodes of inorganic particle stacking network and polymer cross-linked network; utilizes the coordination effect of fullerene and the encapsulation effect of cyclodextrin to delay the reaction time of Pt catalyst, ensure the uniformity of filling process, improve the compactness and uniformity of inorganic thermal conductive network, and obtains a bonding structure with outstanding hardness, elasticity, mechanical strength and thermal conductivity after thermosetting molding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor packaging materials, in particular to a high thermal conductivity filling adhesive for semiconductor flip chip packaging. Background Art

[0002] Flip Chip means connecting the contact points of the chip to the substrate, carrier, or circuit board. During the connection process, the bumps of the chip are connected facing downward, so it is called flip chip.

[0003] The last step of the semiconductor flip chip process is to inject the filling glue around the contact points to support the solder joints and seal. The general filling process is to heat the flip chip and the substrate to 70 to 75°C, and use an L-shaped syringe filled with filler to inject the filler in both directions along the edge of the chip; due to the siphon effect of the capillary in the gap, the filler is sucked in and flows toward the center; there are barriers on the edge of the chip to prevent outflow. Some use the method of tilting the substrate to facilitate flow; after filling, the temperature is raised in stages in the oven, and after reaching a curing temperature of about 130°C, it is kept for 3 to 4 hours to achieve complete curing.

[0004] The bottom filler used in semiconductor flip chip technology is generally composed of adhesives, curing agents, fillers and other additives. In order to promote the heat dissipation of electrical contacts, the thermal conductivity of the filler must be improved, and the thermal conductivity of the filler is more dependent on the type and amount of filler used.

[0005] The filler of the bottom filling glue is generally compounded with inorganic oxide, carbide or nitride particles of different sizes. When the filler reaches a certain filling amount, the filler ions stack into a network, which can form a new thermal conductive network structure in the polymer network of the adhesive. Reasonable design can obtain a packaging structure with ultra-high thermal conductivity.

[0006] In addition to meeting the basic bonding packaging and thermal conductivity requirements, the bottom filler also needs to meet sufficient hardness (structural support) and elasticity (structural toughness) and other properties. Existing fillers can often only meet certain properties. For example, when the inorganic filler content in the bottom filler is too high, it is easy to cause poor adhesion, and when the inorganic filler content is too low, it will cause the inability to form an effective inorganic stacking thermal conductive network; for example, when using epoxy resin with higher adhesion, the elasticity and stability after bonding are ignored. Therefore, the semiconductor field urgently needs a new bottom filler with more comprehensive comprehensive performance. Summary of the invention

[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high thermal conductive filling adhesive for semiconductor flip chip packaging.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A high thermal conductive filling adhesive for semiconductor flip chip packaging comprises the following components in parts by weight:

[0010] 100 parts of vinyl-modified alumina, the surface of spherical alumina was modified by vinyl grafting, and the spherical alumina was purchased from Guangdong Oulite New Materials;

[0011] 1.5-2 parts of fullerene, purchased from Alfa in the United States, of which C60 accounts for 98% and the rest is C70. The molecular size of C60 is 0.7nm, which can be used to fill the gaps in the polymer network and the gaps in the inorganic network, thereby improving thermal conductivity and density;

[0012] 10-15 parts of vinyl-terminated silicone oil, with a molecular weight of 6000-8000, a viscosity of 500-800cps, and a vinyl content of 0.9-1.2mol%;

[0013] 2-3 parts of high vinyl silicone oil, molecular weight of 15000-18000, viscosity of 5000-6000cps, vinyl content of 5-6mol%;

[0014] 5-7 parts of hydrogen-containing silicone oil, with a hydrogen content of 4-5 mmol / g and a molecular weight of 8,000-11,000, as a crosslinking agent, undergoes addition crosslinking reaction with vinyl under catalysis to form a crosslinking network;

[0015] 1-2 parts of Pt catalyst, Custer catalyst, used to catalyze the addition reaction of active hydrogen and vinyl.

[0016] Preferably, the particle sizes of spherical alumina are divided into three types: large, medium and small particles of 5-6 μm, 0.8-1.5 μm and 0.1-0.15 μm, wherein the weight ratio of large particle spherical alumina, medium particle spherical alumina and small particle spherical alumina is 1:0.28-0.30:0.1-0.12.

[0017] Furthermore, the screening process of spherical alumina is as follows: alumina of 6-20 μm is ball-milled, and the size ratio of ball-milled zirconium oxide is 60 mm, 10 mm and 1 mm according to the weight ratio of 10: 0.8-0.9: 0.2-0.3, and the obtained powder is subjected to secondary screening, that is, particles larger than 6 μm and particles smaller than 5 μm are filtered out in turn to obtain large-particle spherical alumina of 5-6 μm; the remaining material is ball-milled again (the zirconium oxide size of the ball mill is adjusted, and the size ratio of ball-milled zirconium oxide is 1 mm, 0.2 mm and 0.1 mm according to the weight ratio of 10: 1.2-1.4: 0.5-0.6), and the obtained powder is subjected to secondary screening, that is, particles larger than 1.5 μm and particles smaller than 0.8 μm are filtered out in turn to obtain medium-particle spherical alumina of 0.8-1.5 μm; the remaining material is sieved to obtain small-particle spherical alumina of 0.1-0.15 μm.

[0018] Preferably, the grafting modification process of vinyl-modified alumina is as follows: take alumina and butanol, prepare a suspension system in a ratio of 1g alumina: 50ml butanol, add vinyltrimethoxysilane, the weight ratio of vinyltrimethoxysilane to alumina is 5:1, add ammonia water to adjust the pH to 10, stir the closed system at 45°C for 2h, centrifuge and dry at 120°C to obtain vinyl-grafted alumina, the surface of the vinyl-grafted alumina is methoxy, vinyl and hydroxyl.

[0019] Preferably, the surface of the fullerene is coated with cyclodextrin, and the surface activation process of the fullerene is as follows: fullerene and toluene are dissolved at a weight ratio of 1:10 at 75°C to obtain a fullerene toluene solution, and cyclodextrin and water are dissolved at a weight ratio of 1:10 at 75°C to obtain a cyclodextrin aqueous solution; the cyclodextrin aqueous solution at 75°C is added dropwise to the fullerene toluene solution at 75°C, mixed homogeneously for 10 minutes, cooled to room temperature, aged, and a fluffy sol is obtained at the bottom; the fluffy sol is placed under a vacuum of <0.01MPa and dried at 75°C for 15 minutes to obtain a colloid of a complex of fullerene and cyclodextrin.

[0020] Furthermore, the weight ratio of the cyclodextrin aqueous solution to the fullerene toluene solution is 1-1.5:1.

[0021] Furthermore, the cyclodextrin is β-cyclodextrin or γ-cyclodextrin, purchased from Hubei Jusheng Technology Co., Ltd.

[0022] Preferably, the vinyl-terminated silicone oil includes at least one of vinyl-terminated polydimethylsiloxane (Vi-PDMS) and vinyl-terminated polymethylvinylsiloxane (Vi-PMVS).

[0023] Preferably, the Pt catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a complex of a colorless to pale yellow liquid with a viscosity of 800-1000 mPa.s and a boiling point of 132-135°C.

[0024] The preparation and use process of the aforementioned high thermal conductivity filling glue for semiconductor flip chip packaging includes the following steps:

[0025] S1. Preparation of filling glue:

[0026] The colloid of the complex of fullerene and cyclodextrin is mixed with a Pt catalyst, and then vinyl-modified alumina, terminal vinyl silicone oil and high vinyl silicone oil are added, and mixed at high speed to obtain a slurry precursor. After the slurry precursor is mixed in a homogenizer, it can ensure long-term stability without sedimentation under water-free sealing conditions;

[0027] The slurry precursor is homogeneously mixed with hydrogen-containing silicone oil to obtain a filling glue injection solution;

[0028] S2. Use of filling glue:

[0029] After the bumps of the semiconductor chip are connected to the pads of the substrate by hot pressing (softening and diffusion at 300℃), the newly prepared filling glue injection liquid is quickly heated to 60℃ and stirred at a high speed of 10000r / min for 5 minutes. The viscosity of the filling glue injection liquid is reduced to 300-400cps by heating and shearing, and injected into the gap between the chip bumps and the substrate solder joints through an L-shaped injection gun. At this time, the substrate is ensured to be still located in the heat source of 300℃. Through capillary action, the position between the chip and the substrate is filled within 1 minute. It becomes viscous after 5 minutes. The excess glue around the chip is cleaned with a scraper, the heat source of the substrate is removed, and the solidified colloid is obtained after natural cooling for 10 minutes, that is, the packaging process is completed, and the thermal conductivity, elasticity, hardness and mechanical strength of the filling glue are tested.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The present invention performs vinyl modification on the surface of aluminum oxide, and rapidly performs catalytic addition reaction of vinyl silicone oil and hydrogen silicone oil under the action of Pt catalyst and by utilizing the heat of the previous step, thereby forming a cross-linked network of inorganic particles and polymer chains interpenetrating each other, and making the inorganic particles not easy to fall off when impacted by external forces (such as pulling or pressure), and obtaining a bonding structure with outstanding hardness, elasticity, mechanical strength and thermal conductivity after thermosetting molding. The filler of the silica gel system is heat-resistant, cold-resistant and flame-resistant (derived from the low glass transition temperature, low expansion when heated, high density and flame retardancy of silica gel), and the durability of semiconductor performance can be guaranteed.

[0032] 2. The present invention utilizes the high reactivity of cyclovinyl groups rich in the surface of fullerene and its active hydrogen with hydrogen-containing silicone oil, so that it can be used as a lubricant (which is beneficial to filling uniformity) and also serve as a node of the inorganic particle stacking network and the polymer cross-linking network, greatly improving the structural stability of the filling glue, further improving the density and uniformity of the inorganic thermal conductive network, and thus improving the thermal conductivity.

[0033] 3. Furthermore, in order to ensure the stability of the catalyst during low-temperature filling, the present invention also utilizes the complexation of fullerene and cyclodextrin (covering part of the surface of the fullerene), the coordination effect of fullerene and the encapsulation effect of cyclodextrin to delay the reaction time of the Pt catalyst, so that the viscosity of the filling glue does not change much during the filling process, thereby further ensuring the filling uniformity. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.

[0035] 1. A formula of a high thermal conductive filler for semiconductor flip chip packaging, comprising the following components in parts by weight:

[0036] 100 parts of vinyl-modified alumina, the surface of spherical alumina is modified by vinyl grafting, the spherical alumina is purchased from Guangdong Oulite New Materials, the particle size of spherical alumina is divided into three types of large, medium and small particles of 5-6μm, 0.8-1.5μm and 0.1-0.15μm, among which the weight ratio of large particle spherical alumina, medium particle spherical alumina and small particle spherical alumina is 1:0.29:0.11;

[0037] 1.5-2 parts of fullerene, purchased from Alfa in the United States, of which C60 accounts for 98% and the rest is C70. The molecular size of C60 is 0.7nm, which can be used to fill the gaps in the polymer network and the gaps in the inorganic network, thereby improving thermal conductivity and density;

[0038] 10-15 parts of vinyl-terminated silicone oil, the vinyl-terminated silicone oil comprising at least one of vinyl-terminated polydimethylsiloxane (Vi-PDMS) and vinyl-terminated polymethylvinylsiloxane (Vi-PMVS), having a molecular weight of 6000-8000, a viscosity of 500-800 cps, and a measured vinyl content of 0.97 mol%;

[0039] 2-3 parts of high vinyl silicone oil, molecular weight of 15000-18000, viscosity of 5000-6000cps, vinyl content of 5.5mol%;

[0040] 5-7 parts of hydrogen-containing silicone oil, with a hydrogen content of 4.2mmol / g and a molecular weight of 8,000-11,000, as a crosslinking agent, undergoes addition crosslinking reaction with vinyl under catalysis to form a crosslinking network;

[0041] 1-2 parts of Pt catalyst, Custer catalyst, Pt catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a colorless to pale yellow liquid complex with a viscosity of 800-1000mPa.s and a boiling point of 132-135°C, and is used to catalyze the addition reaction of active hydrogen and vinyl.

[0042] 2. The preparation process of the aforementioned high thermal conductive filling glue for semiconductor flip chip packaging includes:

[0043] 1) The screening process of spherical alumina is as follows: alumina of 6-20 μm is ball-milled, and the size ratio of ball-milled zirconium oxide is 60 mm, 10 mm and 1 mm according to the weight ratio of 10:0.8-0.9:0.2-0.3, and the obtained powder is subjected to secondary screening, that is, particles larger than 6 μm and particles smaller than 5 μm are filtered out in turn to obtain large-particle spherical alumina of 5-6 μm; the remaining material is ball-milled again (the size of zirconium oxide in the ball mill is adjusted, and the size ratio of ball-milled zirconium oxide is 1 mm, 0.2 mm and 0.1 mm according to the weight ratio of 10:1.2-1.4:0.5-0.6), and the obtained powder is subjected to secondary screening, that is, particles larger than 1.5 μm and particles smaller than 0.8 μm are filtered out in turn to obtain medium-particle spherical alumina of 0.8-1.5 μm; the remaining material is sieved to obtain small-particle spherical alumina of 0.1-0.15 μm.

[0044] 2) The grafting modification process of vinyl-modified alumina is as follows: take alumina and butanol, prepare a suspension system in the ratio of 1g alumina: 50ml butanol, add vinyltrimethoxysilane, the weight ratio of vinyltrimethoxysilane to alumina is 5:1, add ammonia water to adjust the pH to 10, stir the closed system at 45°C for 2h, centrifuge and dry at 120°C to obtain vinyl-grafted alumina, the surface of the vinyl-grafted alumina is methoxy, vinyl and hydroxyl.

[0045] 3) The surface of fullerene is coated with cyclodextrin, and the surface activation process of fullerene is as follows: fullerene and toluene are dissolved at a weight ratio of 1:10 at 75°C to obtain a fullerene toluene solution, and cyclodextrin and water are dissolved at a weight ratio of 1:10 at 75°C to obtain a cyclodextrin aqueous solution; the cyclodextrin aqueous solution at 75°C is added dropwise to the fullerene toluene solution at 75°C, mixed homogeneously for 10 minutes, cooled to room temperature, aged, and a fluffy sol is obtained at the bottom; the fluffy sol is placed under a vacuum of <0.01MPa and dried at 75°C for 15 minutes to obtain a complex colloid of fullerene and cyclodextrin.

[0046] The weight ratio of the cyclodextrin aqueous solution to the fullerene toluene solution is 1-1.5:1.

[0047] Wherein, cyclodextrin is β-cyclodextrin or γ-cyclodextrin, purchased from Hubei Jusheng Technology Co., Ltd.

[0048] 4) Mixing the complex colloid of fullerene and cyclodextrin with the Pt catalyst, adding vinyl-modified alumina, terminal vinyl silicone oil and high vinyl silicone oil, and mixing at high speed to obtain a slurry precursor, which can ensure long-term stability without sedimentation under water-free sealing conditions after mixing in a homogenizer;

[0049] The slurry precursor is homogeneously mixed with hydrogen-containing silicone oil to obtain a filling glue injection solution;

[0050] 3. The encapsulation and use process of the aforementioned filling glue injection is as follows:

[0051] After the bumps of the semiconductor chip are connected to the pads of the substrate by hot pressing (softening and diffusion at 300℃), the newly prepared filling glue injection liquid is quickly heated to 60℃ and stirred at a high speed of 10000r / min for 5 minutes. The viscosity of the filling glue injection liquid is reduced to 300-400cps by heating and shearing, and injected into the gap between the chip bumps and the substrate solder joints through an L-shaped injection gun. At this time, the substrate is ensured to be still located in the heat source of 300℃. Through capillary action, the position between the chip and the substrate is filled within 1 minute. It becomes viscous after 5 minutes. The excess glue around the chip is cleaned with a scraper, the heat source of the substrate is removed, and the solidified colloid is obtained after natural cooling for 10 minutes, that is, the packaging process is completed, and the thermal conductivity, elasticity, hardness and mechanical strength of the filling glue are tested.

[0052] 4. Formulation screening:

[0053] The formula screening is shown in Table 1 below:

[0054] Table 1. Formulation of high thermal conductivity filler for semiconductor flip chip packaging

[0055]

[0056] Comparative Example 6: The formula is the same as that of Example 2, except that the graft-modified spherical alumina is used instead of the vinyl-modified alumina of Example 2;

[0057] Comparative Example 7: The same formulation as Example 2, except that unmodified fullerene powder was used instead of the complex colloid of fullerene and cyclodextrin in Example 2 (based on the same actual content of fullerene);

[0058] Comparative Example 8: The formula is the same as that of Example 2, except that the fullerene powder and the complex colloid of fullerene and cyclodextrin are not added.

[0059] V. Performance test:

[0060] Performance testing includes the following aspects:

[0061] 1) Shore A hardness: according to standard DIN ISO 48-4 ShA / 23°C / t=6mm, 75-80 Shore A;

[0062] 2) Elasticity: 100% deformation tensile modulus (tensilemodolous): 7MPa<TM<12MPa;

[0063] 3) Tear strength: Fix the chip on the test platform with screws, with the substrate located on the upper surface of the chip. Use the translation mechanism to fix the four corners of the substrate with screws and nuts. Drive the translation mechanism to tear the substrate off the chip. The direction of the substrate movement is always on the bonding surface between the chip and the substrate. The force required to separate the substrate from the chip is the tear strength.

[0064] 4) Thermal conductivity: The test standard is ASTM5470.

[0065] 5) Thermal resistance: the test standard is ASTM5470;

[0066] 6) Glass transition temperature: DMA double cantilever mode is used, and the test standard is GB11998-1989;

[0067] 7) Bending strength: The test standard is GB / T2570-1995.

[0068] The test results are shown in Table 2 below:

[0069] Table 2. Performance test of high thermal conductivity filler for semiconductor flip chip packaging

[0070]

[0071] From Comparative Examples 1 to 5, the dosage of vinyl-modified alumina, fullerene, vinyl, active hydrogen and catalyst is too high. The alumina content in Example 2 is 80.6%, while that in the comparative example is as high as 83.3%. Obviously, the inorganic particles are too high, occupying more bonding positions, resulting in reduced bonding properties.

[0072] Comparative Example 2 has a higher fullerene content than Example 2. Fullerene acts as a node of a cross-linked network. It can react with hydrogen-containing silicone oil by using double bonds on its surface ring. On the other hand, it can be used as a lubricant and filler for inorganic particles, which facilitates the neat stacking of inorganic particles and improves the compactness. At the same time, during the heating process, it has sufficient bond tension, greatly reduces the thermal expansion coefficient, and thus ensures the structural stability during the filling and curing process. However, when the dosage is too high (the dosage is too low, it cannot play the role of complex protection catalyst), it is easy to settle and agglomerate and occupy the position of alumina, which makes the thermal conductivity worse and causes too high a cost (fullerene is more expensive).

[0073] The vinyl content of Comparative Example 3 and the hydrogen content of Comparative Example 4 are both too high, resulting in incomplete crosslinking reaction, which is reflected in insufficient hardness and supporting strength;

[0074] During the test, it was found that: through the inclusion effect of cyclodextrin and the coordination effect of fullerene, cross-linking can be effectively prevented under low temperature conditions (<110°C). The present application does not need to add a catalytic retarder, but when the amount of Pt catalyst used is too high (such as in Comparative Example 5), it is easy to cause the catalytic addition reaction to be too fast, which can easily cause cross-linking before the gap between the chip and the substrate is fully filled, thereby greatly reducing the bonding effect.

[0075] Comparative Examples 6-8 show that modification of alumina and fullerene is necessary to enhance the uniformity of the cross-linked network and the inorganic particle stacking network, thereby improving the mechanical properties and thermal conductivity.

[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. High thermal conductivity filling glue for semiconductor flip chip packaging, characterized in that: It includes the following components by weight: 100 parts of vinyl modified spherical alumina; 1.5-2 parts of fullerene; 10-15 parts of vinyl-terminated silicone oil, molecular weight 6000-8000, viscosity 500-800cps, vinyl content 0.9-1.2mol%; 2-3 parts of high vinyl silicone oil, molecular weight of 15000-18000, viscosity of 5000-6000cps, vinyl content of 5-6mol%; 5-7 parts of hydrogen-containing silicone oil, with a hydrogen content of 4-5mmol / g and a molecular weight of 8,000-11,000; 1-2 parts of Pt catalyst, which is a Custer catalyst; The particle sizes of the spherical alumina are divided into three types: large, medium and small particles of 5-6 μm, 0.8-1.5 μm and 0.1-0.15 μm, wherein the weight ratio of large particle spherical alumina, medium particle spherical alumina and small particle spherical alumina is 1:0.28-0.30:0.1-0.12; The grafting modification process of the vinyl-modified spherical alumina is as follows: spherical alumina and butanol are taken, a suspension system is prepared according to the ratio of 1g spherical alumina: 50ml butanol, vinyl trimethoxysilane is added, the weight ratio of vinyl trimethoxysilane to spherical alumina is 5:1, ammonia water is added to adjust the pH to 10, a closed system is stirred at 45°C for 2h, and dried at 120°C after centrifugation to obtain vinyl-grafted spherical alumina; The surface of the fullerene is coated with cyclodextrin, and the surface activation process of the fullerene is as follows: fullerene and toluene are dissolved at a weight ratio of 1:10 at 75°C to obtain a fullerene toluene solution, and cyclodextrin and water are dissolved at a weight ratio of 1:10 at 75°C to obtain a cyclodextrin aqueous solution; the cyclodextrin aqueous solution at 75°C is added dropwise to the fullerene toluene solution at 75°C, homogenized and mixed for 10 minutes, cooled to room temperature, aged, and a fluffy sol is obtained at the bottom; the fluffy sol is placed under a vacuum of <0.01MPa and dried at 75°C for 15 minutes to obtain a colloid of a complex of fullerene and cyclodextrin; The weight ratio of the cyclodextrin aqueous solution to the fullerene toluene solution is 1-1.5:

1.

2. The high thermal conductive filling adhesive for semiconductor flip chip packaging according to claim 1, characterized in that: The screening process of the spherical alumina is as follows: alumina of 6-20 μm is ball-milled, and the ball-milled zirconium oxide size ratio is 60 mm, 10 mm and 1 mm zirconium oxide according to the weight ratio of 10: 0.8-0.9: 0.2-0.3, and particles larger than 6 μm and particles smaller than 5 μm are filtered out in turn to obtain large-particle spherical alumina of 5-6 μm; the remaining material is ball-milled again, and the zirconium oxide size of the ball mill is adjusted. The ball-milled zirconium oxide size ratio is 1 mm, 0.2 mm and 0.1 mm zirconium oxide according to the weight ratio of 10: 1.2-1.4: 0.5-0.6, and particles larger than 1.5 μm and particles smaller than 0.8 μm are filtered out in turn to obtain medium-particle spherical alumina of 0.8-1.5 μm; the remaining material is sieved to obtain small-particle spherical alumina of 0.1-0.15 μm.

3. The high thermal conductive filling adhesive for semiconductor flip chip packaging according to claim 1, characterized in that: The vinyl-terminated silicone oil includes at least one of vinyl-terminated polydimethylsiloxane and vinyl-terminated polymethylvinylsiloxane.

4. The high thermal conductive filling adhesive for semiconductor flip chip packaging according to claim 1, characterized in that: The Pt catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a complex having a viscosity of 800-1000 mPa.s, a boiling point of 132-135° C., and is a colorless to light yellow liquid.

5. The method for preparing the high thermal conductive filling adhesive for semiconductor flip chip packaging according to claim 1, characterized in that: The following steps are involved: The colloid of the complex of fullerene and cyclodextrin is mixed with a Pt catalyst, and then vinyl-modified spherical alumina, terminal vinyl silicone oil and high vinyl silicone oil are added, and mixed at high speed to obtain a slurry precursor. After the slurry precursor is mixed in a homogenizer, it can ensure long-term stability without sedimentation under water-free sealing conditions; The slurry precursor is homogeneously mixed with hydrogen-containing silicone oil to obtain a filling glue injection solution.

6. Application of the filling glue injection obtained by the preparation method according to claim 5 in semiconductor flip chip packaging, characterized in that: The following steps are involved: After the bumps of the semiconductor chip are hot-pressed to the pads of the substrate, the newly prepared filling glue injection liquid is quickly heated to 60°C and stirred at a high speed of 10,000 r / min for 5 minutes. The viscosity of the filling glue injection liquid is reduced to 300-400cps by heating and shearing, and injected into the gap between the chip bumps and the substrate solder joints through an L-shaped injection gun. At this time, the substrate is ensured to be 300°C. Through capillary action, the position between the chip and the substrate is filled within 1 minute. It becomes viscous after 5 minutes. Use a scraper to clean the excess glue around the chip, remove the heat source of the substrate, and naturally cool for 10 minutes to obtain a solidified colloid, completing the packaging process.

Citation Information

Patent Citations

  • Halogen-free flame-retardant addition type organosilicon potting compound for electronic appliances

    CN102408869A

  • Halogen-free high-flame retardance addition type heat conduction silicon rubber adhesive

    CN103045158A

  • Liquid silicone rubber compound

    CN105778513A

  • Condensed type organic silicon pouring sealant and preparation method thereof

    CN116144316A

  • Dispersant for nanocarbon and nanocarbon dispersion

    JP2012213701A