A perovskite film with high luminous efficiency and stability and preparation method thereof

By spin-coating and annealing CsPbBr3 quantum dots with p-MSB solution to form a nanosheet film, the stability problem of the CsPbBr3 quantum dot film in a humidity environment was solved, achieving both high fluorescence quantum yield and humidity stability.

CN117925230BActive Publication Date: 2024-10-01WUHAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310585968.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-10-01
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

It is difficult for CsPbBr3 quantum dot films to have both high fluorescence quantum yield and high stability at the same time. It is especially susceptible to erosion in a humid environment. Existing technologies have tried to construct shells or blocking matrices, but the results have been limited.

Method used

CsPbBr3 quantum dots are mixed with p-MSB solution, spin-coated on a SiO2 glass substrate to form a nanosheet film, and annealed at 80°C. Repeat spin-coating and annealing several times to improve the film's fluorescence quantum yield and humidity stability. .

Benefits of technology

Achieved high fluorescence quantum yield and excellent humidity stability of CsPbBr3 quantum dot/p-MSB nanosheet film. The electron migration rate of p-MSB is much greater than the hole migration rate of CsPbBr3, forming a barrier to prevent moisture erosion and significantly improving fluorescence. quantum yield and maintain stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117925230B_ABST
    Figure CN117925230B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of luminescent materials technology and discloses a perovskite thin film with both high luminous efficiency and stability, as well as its preparation method. The method includes the following steps: uniformly mixing CsPbBr3 quantum dots and p-MSB solution to obtain a CsPbBr3 quantum dot / p-MSB nanosheet solution; spin-coating the mixed nanosheet solution onto the surface of a treated SiO2 glass substrate to form a nanosheet thin film; annealing at 80°C; and repeating the spin-coating and annealing process 3-5 times before annealing again to obtain the perovskite thin film. This invention significantly improves the fluorescence quantum yield by forming a type II heterostructure with p-MSB and CsPbBr3. The hydrophobic p-MSB attached to the CsPbBr3 surface effectively prevents moisture from eroding the CsPbBr3 quantum dots, thus achieving excellent humidity stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to a perovskite film having high luminescent efficiency and stability and a preparation method thereof. Background Art

[0002] In recent years, metal halide perovskites are promising optoelectronic materials that can be used as light-emitting materials for light-emitting diodes and gain media in semiconductor lasers due to their extremely high fluorescence quantum yield, narrow emission bandwidth, excellent exciton binding energy and large absorption coefficient.

[0003] As a typical metal halide perovskite, CsPbBr3 quantum dots can emit green light with extremely high color purity, and the fluorescence quantum yield of CsPbBr3 quantum dot solution is close to 100%. However, the agglomeration of nanocrystals will reduce the fluorescence quantum yield of CsPbBr3 quantum dot film to 18%, which is related to the loss of quantum confinement. At the same time, due to the low formation energy and a large number of surface traps, perovskites are generally susceptible to humidity, which hinders the further application of perovskites in underwater environments. Therefore, how to improve the humidity stability of CsPbBr3 quantum dot films while maintaining a high fluorescence quantum yield remains an important issue.

[0004] At present, more and more studies are trying to explore a method that can effectively improve the stability of CsPbBr3 quantum dots. A conventional method is to construct a relatively inert shell or blocking matrix on the quantum dots to prevent adverse erosion by moisture. The CsPbBr3@CdS core-shell structure effectively improves the stability, but the fluorescence quantum yield is reduced. When SiO2 is used as the shell, the fluorescence quantum yield is improved, but due to lattice mismatch, the surface of CsPbBr3@SiO2 is porous and is still corroded by moisture. In order to solve the problem of lattice mismatch, the CsPbBr3@CsPbBrx structure was proposed, which successfully improved the fluorescence quantum yield, but CsPbBr x The instability of CsPbBr3 quantum dots is still an unresolved issue. CsPbBr3 quantum dots can also be filled into cross-linked polystyrene beads, which show extraordinary waterproof properties. However, since organic matrices such as polystyrene cannot emit light themselves, the effective light-emitting area is sacrificed, which in turn causes the radiation to be attenuated.

[0005] Through the above analysis, the problems and defects of the prior art are: CsPbBr3 quantum dot film cannot have both high fluorescence quantum yield and high stability. Summary of the invention

[0006] The purpose of the present invention is to provide a perovskite film with high luminescence efficiency and stability and a preparation method thereof, in order to address the problem that the existing CsPbBr3 quantum dot film cannot have both high fluorescence quantum yield and high stability.

[0007] In order to achieve the above purpose, the technical solution adopted in this application is:

[0008] The first object of the present invention is to provide a method for preparing a perovskite film with high luminous efficiency and stability, comprising the following steps: uniformly mixing CsPbBr3 quantum dots and p-MSB solution to obtain a CsPbBr3 quantum dots / p-MSB nanosheet solution, spin coating the nanosheet solution on a treated SiO2 glass substrate surface to form a nanosheet film, annealing at 80°C, and repeating the spin coating and annealing 3-5 times to obtain a perovskite film.

[0009] Preferably, the CsPbBr3 quantum dots are prepared according to the following steps:

[0010] S1, dissolving PbBr2 powder in a first solvent to obtain a PbBr2 solution; dissolving Cs2CO3 powder in propionic acid, and subjecting the mixture to ultrasonic treatment to obtain Cs + Precursor solution;

[0011] S2, Cs + After the precursor solution is added to the second solvent and stirred, the PbBr2 solution is injected, and the solution is centrifuged at 1500 r / min and 2000 r / min respectively to remove the supernatant to obtain CsPbBr3 quantum dots.

[0012] Preferably, the mass volume ratio of the PbBr2 and the first solvent is 0.9175 g:5 mL, the first solvent is a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1, and the mass volume ratio of Cs2CO3 and propionic acid is 0.5868 g:1 mL.

[0013] Preferably, the Cs + The volume ratio of the precursor solution, the second solvent and the PbBr2 solution is 25 μL:15 mL:0.27 mL, and the second solvent is a mixed solution of isopropanol and n-hexane in a volume ratio of 1:2.

[0014] Preferably, the mass volume ratio of PbBr2 and p-MSB solution in the CsPbBr3 quantum dots is 0.9175g:8mL.

[0015] Preferably, the p-MSB solution is a p-MSB toluene solution, and the concentration of p-MSB is 0.025-2 mg / mL.

[0016] Preferably, the volume of the nanosheet solution spin-coated is 120-200 μL.

[0017] Preferably, the spin coating method is to rotate the nanosheet solution on the SiO2 glass substrate at 500 r / min for 20 seconds and then at 2000 r / min for another 40 seconds. The annealing time is 1 minute, and the last annealing time is 5 minutes.

[0018] Preferably, the SiO2 glass substrate is processed by first using a cleaning agent to remove oil stains on the surface of the SiO2 glass, then using water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally drying with nitrogen for standby use.

[0019] The second object of the present invention is to provide a perovskite film prepared by the above preparation method having high luminous efficiency and stability.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention provides a perovskite film with high luminescence efficiency and stability. The zero-dimensional-two-dimensional CsPbBr3 quantum dot / p-MSB nanosheet film has higher fluorescence quantum yield and excellent humidity stability. p-MSB and CsPbBr3 form a typical type II heterostructure, and the electron migration rate of p-MSB is much greater than the hole migration rate of CsPbBr3. A large number of additional electrons are transferred to CsPbBr3, and the radiation recombination of CsPbBr3 is enhanced, thereby significantly improving the fluorescence quantum yield. At the same time, the hydrophobic p-MSB is attached to the surface of CsPbBr3, forming a solid barrier that can effectively prevent moisture from corroding the CsPbBr3 quantum dots, thereby obtaining excellent humidity stability.

[0022] (2) The perovskite film with high luminous efficiency and stability provided by the present invention has a simple production process and strong repeatability; it can be prepared in an air environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The process flow chart of the perovskite film with high luminous efficiency and stability of the present invention;

[0024] Figure 2 The normalized photoluminescence spectra of the perovskite films prepared in Examples 1-6 of the present invention and Comparative Example 1;

[0025] Figure 3 The fluorescence quantum yield changes of the perovskite films prepared in Examples 1-6 of the present invention and Comparative Example 1;

[0026] Figure 4The photoluminescence intensity changes of the perovskite films prepared in Example 2 of the present invention and Comparative Example 1 at relative humidity of 30%, 75% and 84%. DETAILED DESCRIPTION

[0027] The following will combine the data in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods. The p-MSB used in the present invention is 1,4-bis(4-methylphenylvinyl)benzene.

[0029] Example 1

[0030] A method for preparing a perovskite film with high luminous efficiency and stability. The process flow chart of the perovskite film is as follows: Figure 1 As shown, the following steps are included:

[0031] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0032] S2, preparation of CsPbBr3 quantum dots: 0.9175g of PbBr2 powder was dissolved in 5mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868g of Cs2CO3 powder was dissolved in 1mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0033] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0034] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 2 mg / mL;

[0035] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0036] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 1 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 38.82%.

[0037] Example 2

[0038] A method for preparing a perovskite film with high luminous efficiency and stability comprises the following steps:

[0039] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0040] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0041] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0042] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 1 mg / mL;

[0043] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0044] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 2 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 39.79%.

[0045] Example 3

[0046] A method for preparing a perovskite film with high luminous efficiency and stability comprises the following steps:

[0047] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0048] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0049] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0050] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 0.5 mg / mL;

[0051] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0052] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 3 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 29.68%.

[0053] Example 4

[0054] A method for preparing a perovskite film with high luminous efficiency and stability comprises the following steps:

[0055] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0056] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0057] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0058] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 0.1 mg / mL;

[0059] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0060] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 4 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 27.82%.

[0061] Example 5

[0062] A method for preparing a perovskite film with high luminous efficiency and stability comprises the following steps:

[0063] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0064] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0065] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0066] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 0.05 mg / mL;

[0067] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0068] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 5 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 24.40%.

[0069] Example 6

[0070] A method for preparing a perovskite film with high luminous efficiency and stability comprises the following steps:

[0071] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0072] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0073] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0074] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 0.025 mg / mL;

[0075] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0076] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Example 6 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 23.55%.

[0077] Comparative Example 1

[0078] A method for preparing a perovskite film comprises the following steps:

[0079] S1. Cleaning of SiO2 glass substrate: Use detergent to clean the oil stains on the surface of SiO2 glass, then use deionized water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use;

[0080] S2. Preparation of CsPbBr3 quantum dots: 0.9175 g of PbBr2 powder was dissolved in 5 mL of a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1 to obtain a PbBr2 solution; 0.5868 g of Cs2CO3 powder was dissolved in 1 mL of propionic acid and subjected to ultrasonic treatment to obtain Cs + Precursor solution;

[0081] 25 μL Cs + The precursor was injected into a mixture of 5 mL of isopropanol and 10 mL of n-hexane. After vigorous stirring for 2 minutes, 0.27 mL of PbBr2 solution was quickly injected into the mixture. The mixture was centrifuged at 1500 r / min and 2000 r / min for two minutes respectively. After removing the supernatant, CsPbBr3 quantum dots were obtained.

[0082] S3, preparation of CsPbBr3 quantum dots / p-MSB nanosheet solution: dissolving the synthesized CsPbBr3 quantum dots in 8 mL of p-MSB toluene solution with a p-MSB concentration of 0 mg / mL;

[0083] S4. Preparation of CsPbBr3 quantum dot / p-MSB nanosheet film: Place a glass substrate on a spin coater, drop the mixed CsPbBr3 quantum dot / p-MSB nanosheet solution on the surface of the glass substrate, set the rotation speed to 500r / min for 20s and then change to 2000r / min for 40s. After spin coating, anneal at 80℃ for 1min. Repeat the above steps 3 times. After the last spin coating, anneal at 80℃ for 5min.

[0084] The CsPbBr3 quantum dot / p-MSB nanosheet film prepared in Comparative Example 1 was tested with an excitation wavelength of 350 nm. The results showed that the fluorescence quantum yield was 18.58%.

[0085] The luminous efficiency and stability performance of the perovskite films prepared in Examples 1-6 and Comparative Example 1 were tested.

[0086] Figure 2 The normalized fluorescence emission spectra (PL) of the perovskite films prepared in Example 2 of the present invention and Comparative Example 1 are shown in FIG. Figure 2 As shown, at an annealing temperature of 80°C, when doped with 1 mg / mL p-MSB (Example 2), the PL intensity is higher than that of undoped p-MSB (Comparative Example 1).

[0087] Figure 3 The fluorescence quantum yield (PLQY) of the perovskite film prepared in Examples 1-6 of the present invention and Comparative Example 1 changes. Figure 3 As shown, the fluorescence quantum yield (PLQY) of the quantum dot film doped with p-MSB (Comparative Example 1) is 23.55%. As the p-MSB doping concentration increases, the PLQY increases. When doped with 1 mg / mL p-MSB toluene solution (Example 2), the PLQY is as high as 39.79%, which is twice as high as that of the undoped (Comparative Example 1). As the doping concentration further increases (Example 1), the PLQY decreases. It shows that 1 mg / mL is the optimal doping concentration.

[0088] After the perovskite film prepared in Example 2 was placed in the atmosphere for one month, the PL had almost no decay, which indicates that the CsPbBr3 quantum dot / p-MSB nanosheet film prepared in the present invention has excellent time stability.

[0089] The films prepared in Example 2 and Comparative Example 1 were exposed to environments with relative humidity of 30%, 75% and 84% for 12 h, respectively. The PL intensity changes were as follows: Figure 4 As shown, Figure 4 The photoluminescence intensity changes of the perovskite films prepared in Example 2 of the present invention and Comparative Example 1 at relative humidity of 30%, 75% and 84%. Figure 4As shown, compared with undoped p-MSB (Comparative Example 1), the CsPbBr3 quantum dots / p-MSB nanosheet film (Example 2) generated by doping 1 mg / mL of p-MSB toluene solution has excellent humidity stability.

[0090] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0091] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a perovskite film having both high luminous efficiency and stability, characterized in that: The following steps are involved: The CsPbBr3 quantum dots and p-MSB solution are uniformly mixed to obtain a CsPbBr3 quantum dots / p-MSB nanosheet solution, the nanosheet solution is spin-coated on the surface of the treated SiO2 glass substrate to form a nanosheet film, and after annealing at 80°C, the spin coating and annealing are repeated 3-5 times to obtain a perovskite film; p-MSB is 1,4-bis(4-methylphenylvinyl)benzene; The treatment method of the SiO2 glass substrate is as follows: first use a cleaning agent to remove oil stains on the surface of the SiO2 glass, then use water, ethanol and acetone for ultrasonic treatment for 10 minutes in sequence, and finally blow dry with nitrogen for standby use.

2. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 1, characterized in that: The CsPbBr3 quantum dots are prepared according to the following steps: S1, dissolving PbBr2 powder in a first solvent to obtain a PbBr2 solution; dissolving Cs2CO3 powder in propionic acid, and subjecting it to ultrasonic treatment to obtain Cs + Precursor solution; S2, Cs + After the precursor solution is added to the second solvent and stirred, the PbBr2 solution is injected, and the solution is centrifuged at 1500 r / min and 2000 r / min respectively to remove the supernatant to obtain CsPbBr3 quantum dots.

3. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 2, characterized in that: The mass volume ratio of the PbBr2 and the first solvent is 0.9175 g:5 mL, the first solvent is a mixed solution of butylamine, isopropanol and propionic acid in a volume ratio of 1:1:1, and the mass volume ratio of the Cs2CO3 and propionic acid is 0.5868 g:1 mL.

4. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 3, characterized in that: The Cs + The volume ratio of the precursor solution, the second solvent and the PbBr2 solution is 25 μL:15 mL:0.27 mL, and the second solvent is a mixed solution of isopropanol and n-hexane in a volume ratio of 1:

2.

5. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 4, characterized in that: The mass volume ratio of PbBr2 and p-MSB solution in the CsPbBr3 quantum dots is 0.9175g:8mL.

6. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 5, characterized in that: The p-MSB solution is a p-MSB toluene solution, and the concentration of p-MSB is 0.025-2 mg / mL.

7. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 1, characterized in that: The volume of the nanosheet solution spin-coated is 120-200 μL.

8. The method for preparing a perovskite film having high luminous efficiency and stability according to claim 1, characterized in that: The spin coating method is to rotate the nanosheet solution on the SiO2 glass substrate at 500 r / min for 20 seconds and then at 2000 r / min for another 40 seconds. The annealing time is 1 minute, and the last annealing time is 5 minutes.

9. A perovskite film having high luminous efficiency and stability prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Bipolar organic single crystal grown by molecular blending, preparation method and application thereof

    CN111926389A

  • Composite electron transport layer with efficient charge extraction and application thereof in perovskite solar cell

    CN113097386A

  • Organic light emitting device

    KR1020130111483A

  • Perovskite color converter and method of manufacturing the same

    US20220145174A1