Thermal conductivity testing method and system of thermal interface materials based on thermal testing chip
Through a method based on thermal testing chip, the working environment of real electronic equipment is simulated and the thermal conductivity of TIM materials is measured, which solves the problem of differences in the test results and actual performance in the prior art, and achieves more accurate thermal conductivity measurement and materials optimization.
Patent Information
- Application Number
- CN202410120945.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-29
AI Technical Summary
Existing thermal conductivity testing methods are usually carried out under ideal or standardized conditions, ignoring the contact thermal resistance and complex thermodynamic processes in real applications, resulting in differences in test results from actual performance, making it difficult to simulate the actual working environment and ensure the test results. Repeatability.
Using a thermal test chip-based method, by preparing thermal test chips and heat sinks, combining thermistors and diodes, simulate the working environment of real electronic equipment, measure the thermal conductivity of TIM materials, consider contact thermal resistance and other factors, and provide more Close to the actual application test environment.
Achieve more accurate measurement of the actual thermal conductivity of TIM materials, reduce performance differences between testing and actual applications under ideal conditions, improve R&D efficiency, reduce costs, and provide more comprehensive data support to help select and optimize TIM material.
Smart Images

Figure CN117929465B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of advanced packaging test technology, and in particular to a thermal conductivity test method and system for a thermal interface material based on a thermal test chip. Background Art
[0002] Thermal interface materials (TIMs) play a vital role in the heat dissipation management of electronic devices. They transfer heat between devices to ensure that the devices run at the optimal operating temperature. As the performance of electronic devices continues to improve and their size continues to decrease, effective thermal management becomes increasingly important. In order to meet these needs, the role of thermal interface materials (TIMs) is indispensable. One of the core properties of TIM materials is their thermal conductivity, because it affects the efficiency of heat transfer. In order to ensure that the performance of TIM materials meets the expected standards, its thermal conductivity needs to be accurately measured.
[0003] However, traditional thermal conductivity testing methods are usually performed under ideal or standardized conditions, which usually ignores various challenges that may arise in real applications, especially the problem of contact thermal resistance, and cannot truly reflect the performance of TIM materials under actual working environments; contact thermal resistance is caused by imperfect interface contact and microscopic inhomogeneity, which can significantly affect the effective thermal conductivity of TIM materials. Under ideal testing conditions, this effect may be ignored, resulting in differences between test results and performance in actual applications, which leads to a dilemma: although the thermal conductivity values tested under ideal conditions may be high, in real applications, these TIM materials may not achieve the expected performance; currently, the main challenges faced in accurately testing the thermal conductivity of TIM materials are how to simulate the actual working environment and conditions, and how to ensure the consistency and repeatability of test results. Many existing testing methods do not fully consider the thermal resistance, thermal diffusion and other complex thermodynamic processes that materials may encounter in real applications.
[0004] On the other hand, in many practical applications, the effectiveness of thermal interface materials (TIM) does not depend solely on their inherent thermal conductivity. Contact thermal resistance, material application thickness, and other factors under real working conditions may have an important impact on the performance of TIM, which also means that the theoretical thermal conductivity value may not fully reflect the effect of TIM in practical applications.
[0005] Therefore, in view of the above problems, the present invention urgently needs to provide a thermal conductivity testing method and system for thermal interface materials based on a thermal testing chip. Summary of the invention
[0006] The purpose of the present invention is to provide a thermal conductivity testing method and system based on a thermal testing chip, which can solve the problem that the existing technology can only be performed under ideal or standardized conditions by simulating the real working environment of electronic equipment.
[0007] The present invention provides a thermal conductivity testing method for a thermal interface material based on a thermal testing chip, comprising the following steps:
[0008] 1) preparing a thermal test chip, the thermal test chip is composed of a plurality of closely arranged chip modules, each of the chip modules comprises a substrate, the upper surface of the substrate is provided with two rows of contacts arranged at intervals, and each contact is respectively connected with a diode CH for temperature measurement, a diode AEFJ and a thermal resistor BI and a thermal resistor DG for heating;
[0009] 2) Prepare a heat sink, attach the upper surface of the thermal test chip to the TIM material, place the heat sink on the TIM material, and sinter and package; electrically connect the electrode pins of the thermal test chip to the thermal conductivity tester, and attach the lower surface of the thermal test chip to the heat sink to obtain a test piece;
[0010] 3) Thermistors are longitudinally installed in the center of the upper and lower heat sinks, so that one end of the thermistor installed on the upper heat sink contacts the surface of the thermal test chip, and one end of the thermistor installed on the lower heat sink contacts the surface of the TIM material; each thermistor is electrically connected to a thermal conductivity tester;
[0011] 4) Start the thermal conductivity tester, apply a fixed voltage and current to the thermal test chip, so that the thermal resistor BI and the thermal resistor DG heat the thermal test chip, the diode CH and the diode AEFJ measure the temperature of the thermal test chip, and obtain the temperature of the thermal test chip and the surface of the TIM material through each thermistor;
[0012] 5) When the temperatures measured by the thermistors, diodes CH and diodes AEFJ are stable, read the temperature values measured by the thermistors, diodes CH and diodes AEFJ, and obtain the thermal conductivity of the TIM material according to the thermal conductivity formula;
[0013] The thermal conductivity formula is:
[0014] Wherein, V is the fixed voltage applied by the thermal conductivity tester to the thermal test chip, I is the fixed current applied by the thermal conductivity tester to the thermal test chip, and λ C is the thermal conductivity of the thermal test chip, A is the effective area of the TIM material, T1 is the temperature of the thermal test chip, T0 is the temperature measured by the thermistor installed on the upper heat sink, d0 is the thickness of the thermal test chip, d is the thickness of the TIM material, and T2 is the temperature measured by the thermistor installed on the lower heat sink; λTIM is the thermal conductivity of the TIM material.
[0015] Preferably, the temperature T1 of the thermal test chip is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the PN junction inside the diode CH under constant power, that is, the K coefficient curve.
[0016] Preferably, the heat sink comprises a copper substrate, a plurality of cooling holes penetrating the copper substrate are arranged at intervals on the side of the copper substrate, an air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device.
[0017] Preferably, each thermistor is an NTC thermistor.
[0018] Preferably, the thermal conductivity tester comprises:
[0019] A chip power supply module, used to apply a fixed voltage and current to the thermal test chip;
[0020] Temperature acquisition module, used to collect temperature data of each thermistor;
[0021] The thermal conductivity calculation module is used to calculate the thermal conductivity of the TIM material according to the temperature data.
[0022] The present invention also provides a thermal conductivity testing method of a thermal interface material based on a thermal testing chip, comprising the following steps:
[0023] 1) preparing a thermal test chip, the thermal test chip is composed of a plurality of closely arranged chip modules, each of the chip modules comprises a substrate, the upper surface of the substrate is provided with two rows of contacts arranged at intervals, and each contact is respectively connected with a diode CH for temperature measurement, a diode AEFJ and a thermal resistor BI and a thermal resistor DG for heating;
[0024] 2) preparing a heat sink, laminating the upper surface of the thermal test chip with the TIM material, placing the heat sink on the TIM material, and sintering and packaging; electrically connecting the electrode pins of the thermal test chip with the thermal conductivity tester, and coating the lower surface of the thermal test chip with a thermal insulation coating to obtain a test piece;
[0025] 3) A thermistor is installed longitudinally in the center of the heat sink so that one end of the thermistor contacts the surface of the TIM material and the thermistor is electrically connected to the thermal conductivity tester;
[0026] 4) Start the thermal conductivity tester, apply a fixed voltage and current to the thermal test chip, so that the thermal resistor BI and the thermal resistor DG heat the thermal test chip, the diode CH and the diode AEFJ measure the temperature of the thermal test chip, and obtain the temperature of the TIM material surface through the thermistor;
[0027] 5) When the temperatures measured by the thermistor, diode CH and diode AEFJ are stable, read the temperature values measured by the thermistor, diode CH and diode AEFJ, and obtain the thermal conductivity of the TIM material according to the thermal conductivity formula;
[0028] The thermal conductivity formula is: TIM =[(V×I)×d] / [A×(T1-T2)];
[0029] Wherein, V is the fixed voltage applied by the thermal conductivity test system to the thermal test chip, I is the fixed current applied by the thermal conductivity test system to the thermal test chip, d is the thickness of the TIM material, A is the effective area of the TIM material, T1 is the temperature of the thermal test chip, and T2 is the temperature measured by the thermistor; λ TIM is the thermal conductivity of the TIM material.
[0030] Preferably, the temperature T1 of the thermal test chip is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the PN junction inside the diode CH under constant power, that is, the K coefficient curve.
[0031] Preferably, the heat sink comprises a copper substrate, a plurality of cooling holes penetrating the copper substrate are arranged at intervals on the side of the copper substrate, an air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device.
[0032] The present invention also provides a thermal conductivity testing system based on the thermal conductivity testing method of the thermal interface material based on the thermal testing chip as described above, comprising:
[0033] Thermal conductivity tester, used to apply fixed voltage and current to the thermal test chip, collect temperature data of each thermistor, and calculate the thermal conductivity of the TIM material based on the temperature data;
[0034] A thermal test chip for providing a heat source;
[0035] A heat sink is used to dissipate heat from the thermal test chip;
[0036] Thermistors are used to collect temperature data of thermal test chips and TIM materials.
[0037] The present invention also provides a thermal conductivity testing system based on the thermal conductivity testing method of the thermal interface material based on the thermal testing chip as described above, comprising:
[0038] Thermal conductivity tester, used to apply fixed voltage and current to the thermal test chip, collect temperature data of each thermistor, and calculate the thermal conductivity of the TIM material based on the temperature data;
[0039] A thermal test chip for providing a heat source;
[0040] A heat sink is used to dissipate heat from the thermal test chip;
[0041] Thermistors are used to collect temperature data of thermal test chips and TIM materials.
[0042] The thermal conductivity testing method and system of the thermal interface material based on the thermal testing chip provided by the present invention have the following improvements compared with the prior art:
[0043] 1. The present invention provides a thermal conductivity testing method and system for thermal interface materials based on a thermal test chip. The present invention provides an innovative testing method for the performance evaluation of thermal interface materials that is closer to the actual application environment. The method takes into account all the thermodynamic processes and various complex factors of the chip in the actual working environment, especially the influence of contact thermal resistance. The thermal test chip is used to simulate the actual working environment, thereby providing a more realistic testing environment for TIM materials, so that researchers and engineers can test the performance of TIM materials under conditions close to the actual application conditions, which not only helps to better select and optimize TIM materials, but also provides valuable data for further research and development. The method can more accurately measure and reflect the actual thermal conductivity of TIM materials, and provide more accurate data and insights for the heat dissipation design and optimization of electronic equipment. Moreover, since the test is closer to the actual application environment, the rework and retesting caused by the performance difference between the data obtained under ideal conditions and the actual application can be reduced, thereby improving the R&D efficiency, reducing unnecessary repeated testing and rework, and reducing the R&D cost. At the same time, accurate data is provided to engineers, which helps to more accurately select materials and reduce material costs.
[0044] 2. The present invention can modularly customize the thermal test chip to simulate various actual application scenarios. The thermal performance of TIM materials of different areas in real applications can be simulated by changing the size of the heating area on the chip. This method can not only provide information about the inherent thermal conductivity of the TIM material, which greatly facilitates the study of the performance of TIM materials under different conditions, but also reveal problems such as contact thermal resistance that may occur in actual applications, providing more comprehensive data support for material selection and optimization. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1It is a structural schematic diagram (cross-sectional view) of a thermal conductivity testing system for a thermal interface material based on a thermal testing chip according to the present invention;
[0047] Figure 2 It is a structural schematic diagram (cross-sectional view) of another thermal conductivity testing system of a thermal interface material based on a thermal testing chip described in the present invention;
[0048] Figure 3 It is a structural schematic diagram (top view) of the thermal test chip described in the present invention;
[0049] Figure 4 It is a structural schematic diagram of the thermal conductivity tester described in the present invention;
[0050] Figure 5 1 is a step diagram of the method for preparing a thermal test chip according to the present invention, wherein (1) is a top view and (2) is a cross-sectional view;
[0051] Figure 6 The figure is a step diagram of the method for preparing the thermal test chip of the present invention, wherein (1) is a top view and (2) is a cross-sectional view.
[0052] Description of reference numerals:
[0053] 2. Thermistor; 3. Thermal test chip; 301. Diode AEFJ; 302. Diode CH; 303. Thermal resistor BI; 304. Thermal resistor DG; 31. P-type region; 32. N-type region; 33. First through hole; 34. First metal layer; 35. Second through hole; 36. Second metal layer; 37. Third metal layer; 38. Fourth metal layer; 39. Substrate; 310. P+ ohmic contact; 311. N+ ohmic contact; 312. Silicon dioxide; 313. Polysilicon; 314. Silicon nitride layer; 4. TIM material; 6. Heat sink; 7. Cooling device; 8. Thermal insulation coating; 9. Thermal conductivity tester. DETAILED DESCRIPTION
[0054] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0056] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0057] like Figure 1 , Figure 3 As shown, this embodiment provides a thermal conductivity testing method of a thermal interface material based on a thermal testing chip, comprising the following steps:
[0058] 1) preparing a thermal test chip 3, the thermal test chip 3 is composed of a plurality of closely arranged chip modules, each of the chip modules comprises a substrate, the upper surface of the substrate is provided with two rows of contacts arranged at intervals, and each contact is respectively connected with a diode CH302 for temperature measurement, a diode AEFJ301, and a thermal resistor BI303 and a thermal resistor DG304 for heating;
[0059] 2) Prepare a heat sink 6, attach the upper surface of the thermal test chip 3 to the TIM material 4, place the heat sink 6 on the TIM material 4, and sinter and package; electrically connect the electrode pins of the thermal test chip 3 to the thermal conductivity tester 9, and attach the lower surface of the thermal test chip 3 to the heat sink 6 to obtain a test piece;
[0060] 3) Thermistors 2 are longitudinally installed in the centers of the upper and lower heat sinks 6, so that one end of the thermistor 2 installed on the upper heat sink contacts the surface of the thermal test chip 3, and one end of the thermistor 2 installed on the lower heat sink contacts the surface of the TIM material 4; each thermistor 2 is electrically connected to a thermal conductivity tester 9;
[0061] 4) Start the thermal conductivity tester 9, apply a fixed voltage and current to the thermal test chip 3, so that the thermal resistor BI303 and the thermal resistor DG304 heat the thermal test chip 3, the diode CH302 and the diode AEFJ301 measure the temperature of the thermal test chip 3, and obtain the temperature of the thermal test chip 3 and the surface of the TIM material 4 through each thermistor 2;
[0062] 5) When the temperatures measured by the thermistor 2, the diode CH302 and the diode AEFJ301 are stable, read the temperature values measured by the thermistor 2, the diode CH302 and the diode AEFJ301, and obtain the thermal conductivity of the TIM material 4 according to the thermal conductivity formula;
[0063] The thermal conductivity formula is:
[0064] Wherein, V is a fixed voltage applied by the thermal conductivity tester 9 to the thermal test chip 3, I is a fixed current applied by the thermal conductivity tester 9 to the thermal test chip 3, and λ C is the thermal conductivity of the thermal test chip 3, A is the effective area of the TIM material 4, T1 is the temperature of the thermal test chip 3, T0 is the temperature measured by the thermistor 2 installed on the upper heat sink, d0 is the thickness of the thermal test chip 3, d is the thickness of the TIM material 4, and T2 is the temperature measured by the thermistor 2 installed on the lower heat sink; λ TIM is the thermal conductivity of the TIM material 4 ; wherein the TIM material 4 completely covers the heat sink 6 , and the effective area A of the TIM material 4 is the area of the heat sink 6 .
[0065] In the thermal test chip 3 of the present invention, the conduction direction of the diode CH points to the contact C, and the positive contacts of the thermal resistor BI and the thermal resistor DG are B and D respectively.
[0066] The present invention provides a thermal conductivity testing method for thermal interface materials based on a thermal test chip, which provides an innovative testing method for the performance evaluation of thermal interface materials that is closer to the actual application environment, takes into account all thermodynamic processes and various complex factors of the chip in the actual working environment, especially the influence of contact thermal resistance, and uses the thermal test chip to simulate the actual working environment, thereby providing a more realistic testing environment for TIM materials, so that researchers and engineers can test the performance of TIM materials under conditions close to the actual application conditions, which not only helps to better select and optimize TIM materials, but also provides valuable data for further research and development, can more accurately measure and reflect the actual thermal conductivity of TIM materials, and provides more accurate data and insights for the heat dissipation design and optimization of electronic equipment; and because the test is closer to the actual application environment, it can reduce rework and retesting caused by the performance difference between data obtained under ideal conditions and actual applications, thereby improving research and development efficiency, reducing unnecessary repeated testing and rework, and reducing research and development costs. At the same time, accurate data is provided to engineers, which helps to more accurately select materials and reduce material costs;
[0067] At the same time, the present invention can modularly customize the thermal test chip to simulate various actual application scenarios. The thermal performance of TIM materials of different areas in real applications can be simulated by changing the size of the heating area on the chip. This method can not only provide information about the inherent thermal conductivity of the TIM material, which greatly facilitates the study of the performance of TIM materials under different conditions, but also reveal problems such as contact thermal resistance that may occur in actual applications, providing more comprehensive data support for material selection and optimization.
[0068] like Figure 5 , Figure 6 As shown, the preparation method of the thermal test chip 3 is as follows: A preparation method of a thermal test chip based on thermal conductivity, characterized in that it includes the following steps:
[0069] Boron ions are implanted at intervals on the left side, the center and the right side of the upper surface of the substrate 39 to form a P-type region 31 of the diode;
[0070] Phosphorus ions are implanted into the P-type region 31 at the center to form an N-type region 32;
[0071] Boron ions are injected into each P-type region 31, so that P+ ohmic contacts 310 are symmetrically formed at the upper and lower ends of each P-type region 31, and two P+ ohmic contacts 310 of the P-type region 31 located at the center of the substrate 39 are arranged on both sides of the N-type region 32;
[0072] Phosphorus ions are implanted into the N-type region 32 to form an N+ ohmic contact 311, and then the substrate 39 is obtained by stripping, cleaning, drying, and thermal annealing.
[0073] Depositing silicon dioxide 312 on the pre-processed substrate 39, coating, exposing, and developing a hard film in sequence to form a first through hole 33 connected to each P+ ohmic contact 310 and N+ ohmic contact 311, and depositing metal on the silicon dioxide 312 and the first through hole 33 to form a first metal layer 34;
[0074] Etching the first metal layer 34 to retain the first metal layer 34 above each P+ ohmic contact 310 and above the N+ ohmic contact 311;
[0075] Depositing silicon dioxide 312 on the silicon dioxide 312 and the first metal layer 34, coating with glue, exposing, and developing a hard film in sequence to form second through holes 35 connected to the first metal layers 34, and depositing metal on the silicon dioxide 312 and the second through holes 35 to form a second metal layer 36;
[0076] According to the circuit layout, mask, etch the second metal layer 36, retain the second metal layer 36 above each first metal layer 34, retain three intervals of the second metal layer 36 in strips, marked as GD connection area, HC connection area, IB connection area, retain the second metal layer 36 on both sides of the HC connection area and located above the N+ ohmic contact 311, retain the first connection area connecting the GD connection area with the second metal layer 36 above the adjacent N+ ohmic contact 311, and the second connection area connecting the IB connection area with the second metal layer 36 above the adjacent N+ ohmic contact 311;
[0077] Depositing silicon nitride on the silicon dioxide 312 and the second metal layer 36 to form a silicon nitride layer 314, coating with glue, exposing, and developing a hard film, exposing the second metal layer 36 at both ends of the left P-type region and the right P-type region, the second metal layer 36 at both ends of the GD wiring region, the second metal layer 36 at both ends of the HC wiring region, and the second metal layer 36 in the IB wiring region;
[0078] Depositing a third metal layer 37 on the silicon nitride layer 314 and the second metal layer 36, etching the third metal layer 37, retaining the third metal layer 37 at both ends of the left P-type region and the right P-type region, marking them as F contact and E contact, J contact and A contact respectively, retaining the third metal layer 37 above both ends of the GD connection region, marking them as G contact and D contact, and the third metal layer 37 above both ends of the HC connection region, marking them as H contact and C contact, retaining the third metal layer 37 above the IB connection region, marking them as I contact and B contact respectively;
[0079] like Figure 5As shown, the back side of the substrate 39 is etched to form lower injection grooves corresponding to the upper and lower sides of the F contact, the E contact, the G contact, the D contact, the H contact, the C contact, the I contact, and the B contact, each lower injection groove is connected to the second metal layer 36, and polysilicon 313 is injected into each lower injection groove;
[0080] like Figure 6 As shown, a fourth metal layer 38 is deposited on the back side of the substrate 39 , and the fourth metal layer 38 is etched to retain the fourth metal layer 38 covering the lower injection groove regions, thereby obtaining a thermal test chip 3 .
[0081] In this embodiment, the temperature T1 of the thermal test chip 3 is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the PN junction inside the diode CH302 under constant power, that is, the K coefficient curve.
[0082] As is known to all, the voltage drop across the PN junction of the diode 302 changes with temperature conditions. Therefore, the temperature T1 of the thermal test chip 3 can be obtained according to the relationship between the junction temperature and the conduction voltage drop of the PN junction of the diode CH302, ie, the K coefficient curve.
[0083] like Figure 1 As shown, the heat sink 6 includes a copper base plate, and a plurality of cooling holes penetrating the copper base plate are arranged at intervals on the side of the copper base plate. An air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device 7.
[0084] In this embodiment, each thermistor 2 is an NTC thermistor.
[0085] In the present invention, the thermistor 2 installed on the upper heat sink is used to measure the temperature of the thermal test chip 3 , and the thermistor 2 installed on the lower heat sink is used to measure the surface temperature of the TIM material 4 .
[0086] like Figure 4 As shown, the thermal conductivity tester 9 comprises:
[0087] A chip power supply module, used for applying a fixed voltage and current to the thermal test chip 3;
[0088] A temperature acquisition module is used to collect temperature data of each thermistor 2;
[0089] A control and thermal conductivity calculation module, for calculating the thermal conductivity of the TIM material 4 according to the temperature data;
[0090] The chip power supply module is electrically connected to the thermal test chip 3 , the temperature acquisition module is electrically connected to each thermistor 2 , and the chip power supply module and the temperature acquisition module are electrically connected to the control and thermal conductivity calculation module respectively.
[0091] The thermal conductivity tester 9 provided by the present invention applies a fixed voltage and current to the thermal test chip 3 through a chip power supply module, collects temperature data measured by each thermistor 2 through a temperature acquisition module, and obtains the thermal conductivity of the thermal interface material according to the experimental data through a thermal conductivity calculation module, thereby reducing unnecessary manual operations and improving research and development efficiency.
[0092] like Figure 2 , Figure 3 As shown, a thermal conductivity testing method of a thermal interface material based on a thermal testing chip is characterized by comprising the following steps:
[0093] 1) preparing a thermal test chip 3, the thermal test chip 3 is composed of a plurality of closely arranged chip modules, each of the chip modules comprises a substrate, the upper surface of the substrate is provided with two rows of contacts arranged at intervals, and each contact is respectively connected with a diode CH302 for temperature measurement, a diode AEFJ301, and a thermal resistor BI303 and a thermal resistor DG304 for heating;
[0094] 2) Prepare a heat sink 6, attach the upper surface of the thermal test chip 3 to the TIM material 4, place the heat sink 6 on the TIM material 4, and sinter and package; electrically connect the electrode pins of the thermal test chip 3 to the thermal conductivity tester 9, and apply a thermal insulation coating 8 on the lower surface of the thermal test chip 3 to obtain a test piece;
[0095] 3) The thermistor 2 is longitudinally installed in the center of the heat sink 6 so that one end of the thermistor 2 contacts the surface of the TIM material 4 and the thermistor 2 is electrically connected to the thermal conductivity tester 9;
[0096] 4) Start the thermal conductivity tester 9, apply a fixed voltage and current to the thermal test chip 3, so that the thermal resistor BI303 and the thermal resistor DG304 heat the thermal test chip 3, the diode CH302 and the diode AEFJ301 measure the temperature of the thermal test chip 3, and obtain the temperature of the surface of the TIM material 4 through the thermistor 2;
[0097] 5) When the temperatures measured by thermistor 2, diode CH302 and diode AEFJ301 are stable, read the temperature values measured by thermistor 2, diode CH302 and diode AEFJ301, and obtain the thermal conductivity of TIM material 4 according to the thermal conductivity formula;
[0098] The thermal conductivity formula is: TIM =[(V×I)×d] / [A×(T1-T2)];
[0099] Wherein, V is a fixed voltage applied by the thermal conductivity test system to the thermal test chip 3, I is a fixed current applied by the thermal conductivity test system to the thermal test chip 3, d is the thickness of the TIM material 4, A is the effective area of the TIM material 4, T1 is the temperature of the thermal test chip 3, and T2 is the temperature measured by the thermistor 2; λ TIM is the thermal conductivity of the TIM material 4 ; wherein the TIM material 4 completely covers the heat sink 6 , and the effective area A of the TIM material 4 is the area of the heat sink 6 .
[0100] In the thermal test chip 3 of the present invention, the conduction direction of the diode CH points to the contact C, and the positive contacts of the thermal resistor BI and the thermal resistor DG are B and D respectively.
[0101] The present invention provides a thermal conductivity testing method for thermal interface materials based on a thermal test chip, which provides an innovative testing method for the performance evaluation of thermal interface materials that is closer to the actual application environment, takes into account all thermodynamic processes and various complex factors of the chip in the actual working environment, especially the influence of contact thermal resistance, and uses the thermal test chip to simulate the actual working environment, thereby providing a more realistic testing environment for TIM materials, so that researchers and engineers can test the performance of TIM materials under conditions close to the actual application conditions, which not only helps to better select and optimize TIM materials, but also provides valuable data for further research and development, can more accurately measure and reflect the actual thermal conductivity of TIM materials, and provides more accurate data and insights for the heat dissipation design and optimization of electronic equipment; and because the test is closer to the actual application environment, it can reduce rework and retesting caused by the performance difference between data obtained under ideal conditions and actual applications, thereby improving research and development efficiency, reducing unnecessary repeated testing and rework, and reducing research and development costs. At the same time, accurate data is provided to engineers, which helps to more accurately select materials and reduce material costs;
[0102] At the same time, the present invention can modularly customize the thermal test chip to simulate various actual application scenarios. The thermal performance of TIM materials of different areas in real applications can be simulated by changing the size of the heating area on the chip. This method can not only provide information about the inherent thermal conductivity of the TIM material, which greatly facilitates the study of the performance of TIM materials under different conditions, but also reveal problems such as contact thermal resistance that may occur in actual applications, providing more comprehensive data support for material selection and optimization.
[0103] In this embodiment, the temperature T1 of the thermal test chip 3 is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the PN junction inside the diode CH302 under constant power, that is, the K coefficient curve.
[0104] like Figure 2As shown, the heat sink 6 includes a copper base plate, and a plurality of cooling holes penetrating the copper base plate are arranged at intervals on the side of the copper base plate. An air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device 7.
[0105] like Figure 1 As shown, the present invention also provides a thermal conductivity testing system based on the thermal conductivity testing method of the thermal interface material based on the thermal testing chip as described above,
[0106] It includes a thermal conductivity tester 9, which is used to apply a fixed voltage and current to the thermal test chip 3, collect temperature data of each thermistor 2, and calculate the thermal conductivity of the TIM material 4 according to the temperature data;
[0107] A thermal test chip 3, used for providing a heat source;
[0108] A heat sink 6, used for dissipating heat from the thermal test chip 3;
[0109] The thermistor 2 is used to collect temperature data of the thermal test chip 3 and the TIM material 4.
[0110] like Figure 2 As shown, the present invention also provides a thermal conductivity testing system based on the thermal conductivity testing method of the thermal interface material based on the thermal testing chip as described above,
[0111] It includes a thermal conductivity tester 9, which is used to apply a fixed voltage and current to the thermal test chip 3, collect temperature data of each thermistor 2, and calculate the thermal conductivity of the TIM material 4 according to the temperature data;
[0112] A thermal test chip 3, used for providing a heat source;
[0113] A heat sink 6, used for dissipating heat from the thermal test chip 3;
[0114] The thermistor 2 is used to collect temperature data of the thermal test chip 3 and the TIM material 4.
[0115] The present invention also provides two embodiments, as described below:
[0116] Specific plan 1:
[0117] 1) preparing a thermal test chip 3;
[0118] 2) Assemble the thermal test chip 3, the heat sink 6 and the TIM material, and electrically connect them to the thermal conductivity tester 9 to obtain a test piece;
[0119] 3) Assembling thermistors 2 and electrically connecting each thermistor 2 to a thermal conductivity tester 9;
[0120] 4) Start the thermal conductivity tester 9;
[0121] 5) When the temperatures measured by the thermistor 2, the diode CH302 and the diode AEFJ301 are stable, read the temperature values measured by the thermistor 2, the diode CH302 and the diode AEFJ301, and obtain the thermal conductivity of the TIM material 4 according to the thermal conductivity formula;
[0122] In this embodiment, the fixed voltage V applied by the thermal conductivity tester 9 to the thermal test chip 3 is 20V, the fixed current I applied by the thermal conductivity tester 9 to the thermal test chip 3 is 2A, and the thermal conductivity λ of the thermal test chip 3 is C is 150W / (m·K), and the effective area of the TIM material 4, i.e., the area A of the heat sink 6, is 1cm 2 , the temperature T1 of the thermal test chip 3 obtained according to the relationship between the junction temperature and the on-state voltage drop of the PN junction is 126°C, the temperature T0 measured by the thermistor 2 installed on the upper heat sink is 124.94°C, the thickness d0 of the thermal test chip 3 is 0.5mm, the thickness d of the TIM material 4 is 0.1mm, and the temperature T2 measured by the thermistor 2 installed on the lower heat sink is 125.94°C;
[0123] The thermal conductivity λ of TIM material 4 is calculated according to the thermal conductivity formula TIM for:
[0124]
[0125] Specific plan 2:
[0126] 1) preparing a thermal test chip 3;
[0127] 2) Assembling the thermal test chip 3, the heat sink 6 and the TIM material, coating the lower surface of the thermal test chip 3 with a thermal insulation coating 8, and electrically connecting it to a thermal conductivity tester 9 to obtain a test piece;
[0128] 3) Assembling thermistors 2 and electrically connecting each thermistor 2 to a thermal conductivity tester 9;
[0129] 4) Start the thermal conductivity tester 9;
[0130] 5) When the temperatures measured by thermistor 2, diode CH302 and diode AEFJ301 are stable, read the temperature values measured by thermistor 2, diode CH302 and diode AEFJ301, and obtain the thermal conductivity of TIM material 4 according to the thermal conductivity formula;
[0131] In this embodiment, the fixed voltage V applied by the thermal conductivity tester 9 to the thermal test chip 3 is 20V, the fixed current I applied by the thermal conductivity tester 9 to the thermal test chip 3 is 2A, the thickness d of the TIM material 4 is 0.1mm, and the effective area of the TIM material 4, that is, the area A of the heat sink 6, is 1cm2 , the temperature T1 of the thermal test chip 3 obtained according to the relationship between the junction temperature and the on-state voltage drop of the PN junction is 100°C, and the temperature T2 measured by the thermistor 2 is 99.71°C;
[0132] The thermal conductivity λ of TIM material 4 is calculated according to the thermal conductivity formula TIM for:
[0133]
[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A thermal conductivity testing method for thermal interface materials based on a thermal testing chip, characterized in that: The steps include: 1) preparing a thermal test chip (3), the thermal test chip (3) being composed of a plurality of closely arranged chip modules, each of the chip modules comprising a substrate, the upper surface of the substrate being provided with two rows of contacts arranged at intervals, each of the contacts being respectively connected with a diode CH (302) for temperature measurement, a diode AEFJ (301) and a thermal resistor BI (303) and a thermal resistor DG (304) for heating; 2) preparing a heat sink (6), laminating the upper surface of the thermal test chip (3) with the TIM material (4), placing the heat sink (6) on the TIM material (4), and sintering and packaging; electrically connecting the electrode pins of the thermal test chip (3) with the thermal conductivity tester (9), and bonding the lower surface of the thermal test chip (3) with the heat sink (6), to obtain a test piece; 3) Thermistors (2) are longitudinally installed in the centers of the upper and lower heat sinks (6), so that one end of the thermistor (2) installed on the upper heat sink contacts the surface of the thermal test chip (3), and one end of the thermistor (2) installed on the lower heat sink contacts the surface of the TIM material (4); each thermistor (2) is electrically connected to a thermal conductivity tester (9) respectively; 4) starting the thermal conductivity tester (9) and applying a fixed voltage and current to the thermal test chip (3), so that the thermal resistor BI (303) and the thermal resistor DG (304) heat the thermal test chip (3), the diode CH (302) and the diode AEFJ (301) measure the temperature of the thermal test chip (3), and the temperature of the thermal test chip (3) and the surface of the TIM material (4) are obtained through the thermistors (2); 5) When the temperatures measured by the thermistors (2), the diodes CH (302) and the diodes AEFJ (301) are stable, the temperature values measured by the thermistors (2), the diodes CH (302) and the diodes AEFJ (301) are read, and the thermal conductivity of the TIM material (4) is obtained according to the thermal conductivity formula; The thermal conductivity formula is: Wherein, V is a fixed voltage applied by the thermal conductivity tester (9) to the thermal test chip (3), I is a fixed current applied by the thermal conductivity tester (9) to the thermal test chip (3), and λ C is the thermal conductivity of the thermal test chip (3), A is the effective area of the TIM material (4), T1 is the temperature of the thermal test chip (3), T0 is the temperature measured by the thermistor (2) installed on the upper heat sink, d0 is the thickness of the thermal test chip (3), d is the thickness of the TIM material (4), and T2 is the temperature measured by the thermistor (2) installed on the lower heat sink; λ TIm is the thermal conductivity of the TIM material (4); The temperature T1 of the thermal test chip (3) is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the internal PN junction of the diode CH (302) under constant power, that is, the K coefficient curve.
2. The thermal conductivity testing method of thermal interface materials based on thermal testing chip according to claim 1, characterized in that: The heat sink (6) comprises a copper base plate, a plurality of cooling holes penetrating the copper base plate are arranged at intervals on the side of the copper base plate, an air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device (7).
3. The thermal conductivity testing method of thermal interface materials based on thermal testing chip according to claim 2, characterized in that: Each thermistor (2) is an NTC thermistor.
4. The thermal conductivity testing method of thermal interface materials based on thermal testing chip according to claim 3, characterized in that: The thermal conductivity tester (9) comprises: A chip power supply module, used for applying a fixed voltage and current to the thermal test chip (3); A temperature acquisition module, used for acquiring temperature data of each thermistor (2); The thermal conductivity calculation module is used to calculate the thermal conductivity of the TIM material (4) according to the temperature data.
5. A thermal conductivity testing method for thermal interface materials based on a thermal testing chip, characterized in that: The steps include: 1) preparing a thermal test chip (3), the thermal test chip (3) being composed of a plurality of closely arranged chip modules, each of the chip modules comprising a substrate, the upper surface of the substrate being provided with two rows of contacts arranged at intervals, each of the contacts being respectively connected with a diode CH (302) for temperature measurement, a diode AEFJ (301) and a thermal resistor BI (303) and a thermal resistor DG (304) for heating; 2) preparing a heat sink (6), laminating the upper surface of the thermal test chip (3) with the TIM material (4), placing the heat sink (6) on the TIM material (4), and sintering and packaging; electrically connecting the electrode pins of the thermal test chip (3) with the thermal conductivity tester (9), and coating the lower surface of the thermal test chip (3) with a thermal insulation coating (8), thereby obtaining a test piece; 3) a thermistor (2) is longitudinally installed in the center of the heat sink (6) so that one end of the thermistor (2) contacts the surface of the TIM material (4), and the thermistor (2) is electrically connected to a thermal conductivity tester (9); 4) starting the thermal conductivity tester (9) and applying a fixed voltage and current to the thermal test chip (3), so that the thermal resistor BI (303) and the thermal resistor DG (304) heat the thermal test chip (3), the diode CH (302) and the diode AEFJ (301) measure the temperature of the thermal test chip (3), and the temperature of the surface of the TIM material (4) is obtained through the thermistor (2); 5) When the temperatures measured by the thermistor (2), the diode CH (302) and the diode AEFJ (301) are stable, the temperature values measured by the thermistor (2), the diode CH (302) and the diode AEFJ (301) are read, and the thermal conductivity of the TIM material (4) is obtained according to the thermal conductivity formula; The thermal conductivity formula is: TIM =[(V×I)×d] / [A×(T1-T2)]; Wherein, V is a fixed voltage applied by the thermal conductivity test system to the thermal test chip (3), I is a fixed current applied by the thermal conductivity test system to the thermal test chip (3), d is the thickness of the TIM material (4), A is the effective area of the TIM material (4), T1 is the temperature of the thermal test chip (3), and T2 is the temperature measured by the thermistor (2); λ TIM is the thermal conductivity of the TIM material (4); The temperature T1 of the thermal test chip (3) is the junction temperature calculated by the relationship between the junction temperature and the conduction voltage drop of the internal PN junction of the diode CH (302) under constant power, that is, the K coefficient curve.
6. The thermal conductivity testing method of thermal interface materials based on thermal testing chip according to claim 5, characterized in that: The heat sink (6) comprises a copper base plate, a plurality of cooling holes penetrating the copper base plate are arranged at intervals on the side of the copper base plate, an air cooling pipe or a water cooling pipe is respectively installed in each cooling hole, and one end of the air cooling pipe or the water cooling pipe is also connected to a cooling device (7).
7. A thermal conductivity testing system based on the thermal conductivity testing method of thermal interface materials based on a thermal testing chip as claimed in any one of claims 1 to 4, characterized in that: It comprises a thermal conductivity tester (9) for applying a fixed voltage and current to a thermal test chip (3), collecting temperature data of each thermistor (2), and calculating the thermal conductivity of the TIM material (4) according to the temperature data; A thermal test chip (3), used for providing a heat source; A heat sink (6) for dissipating heat from the thermal test chip (3); The thermistor (2) is used to collect temperature data on the surface of the thermal test chip (3) and the TIM material (4).
8. A thermal conductivity testing system based on the thermal conductivity testing method of a thermal interface material based on a thermal testing chip as claimed in any one of claims 5 to 6, characterized in that: It comprises a thermal conductivity tester (9) for applying a fixed voltage and current to a thermal test chip (3), collecting temperature data of each thermistor (2), and calculating the thermal conductivity of the TIM material (4) according to the temperature data; A thermal test chip (3), used for providing a heat source; A heat sink (6) for dissipating heat from the thermal test chip (3); The thermistor (2) is used to collect temperature data on the surface of the thermal test chip (3) and the TIM material (4).
Citation Information
Patent Citations
Thermal resistance measuring device and method for heat conduction grease
CN110687159A
Structure and method for measuring heat conductivity of heterojunction interface in dot matrix contact mode
CN113176293A
Method and system for determining thermal resistance of double-sided heat dissipation module
CN115219554A
Contact thermal resistance testing equipment and method for interface material in microsystem package
CN115791883A
Method and system for testing thermal conductivity of thermal interface material and electronic equipment