Heterogeneous metal welding structure and welding and riveting composite connection method

By using prefabricated grooves and brazing-friction stir welding composite connection method in heterogeneous metal welding, the problems of joint strength and stress relief are solved, efficient heterogeneous metal welding is achieved, and welding quality and efficiency are improved.

CN117943724BActive Publication Date: 2024-12-03DALIAN UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410216125.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-27
Publication Date
2024-12-03
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

The existing heterometal welding technology is difficult to simultaneously increase joint strength, reduce intermetallic compound thickness and release residual stress, resulting in limited welding quality and efficiency.

Method used

Using a heterogeneous metal welding structure, a prefabricated groove is provided on the metal plate A. During welding, welding and riveting composite connection method is used to increase the contact area and fill metal through the prefabricated groove, and the brittleness of friction stir welding is used to break The phase is thinned out the thickness of the intermetallic compound and releases residual stress.

Benefits of technology

It significantly improves the strength and mechanical properties of the welded joints, reduces the thickness and brittleness of intermetallic compounds, and improves weld forming and stress release.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117943724B_ABST
    Figure CN117943724B_ABST
Patent Text Reader

Abstract

The present invention discloses a welding structure of heterogeneous metals and a welding and riveting composite connection method thereof. Two heterogeneous metal plates are welded by using fusion brazing combined with stir friction welding. A prefabricated groove is opened on the surface of one of the plates before welding. During welding, the welding gun is started first to fill the prefabricated groove on the surface of the plate with welding wire. When the weld metal is in a semi-solid state, the stirring head of the stir friction welding intervenes, and the welding gun and the stirring head of the stir friction welding move forward synchronously to complete the welding. Through the above technical scheme, the thickness of the intermetallic compound layer of the weld is reduced, and its morphology is changed, effectively releasing the residual stress of the joint; through the design of the prefabricated groove, combined with fusion brazing and stir friction welding, the macro-micro welding and riveting composite connection of the two heterogeneous metal plates is achieved at the same time, which significantly improves the mechanical properties of the joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material connection, and in particular relates to a heterogeneous metal welding structure and a welding and riveting composite connection method. Background Art

[0002] Heterogeneous metal welding refers to the process of connecting two or more different metals (mainly those with large differences in chemical properties and thermophysical properties) under certain process conditions. Heterogeneous metal welded structures can not only bring out the good properties of each parent material, but also reduce costs. However, heterogeneous metal welding also has many difficulties and pain points, and various technical bottlenecks need to be overcome to ensure welding quality and efficiency.

[0003] Taking aluminum alloy and titanium alloy as examples, aluminum-titanium composite structures have the advantages of aluminum's good ductility, low density and good processing formability and titanium's good high temperature resistance and strong corrosion resistance, and are widely used in many fields such as aerospace, navigation, automobiles, and rail transportation. However, the solid solubility of aluminum and titanium in the solid state is limited, and the thermal conductivity, thermal expansion coefficient, etc. are quite different. After welding, the joints are prone to produce a large amount of brittle intermetallic compounds such as TiAl and TiAl3 and large residual stress, resulting in low strength of aluminum-titanium joints. Therefore, it is very important to choose a suitable welding method for connecting aluminum-titanium heterogeneous metals.

[0004] The literature "Influence of welding parameters on the IMCs and the mechanical properties of Ti / Al butt joints welded by MIG / TIG double-sided arc welding-brazing. Y. Zhang, J. Huang, Z. Ye, et al. Journal of Alloys and Compounds, 2018 747: 764-771" reported a method of realizing Ti / Al connection by MIG-TIG double-sided brazing. This process is difficult to control the heat input, and the heat distribution of the joint is uneven, resulting in different thicknesses of the intermetallic compounds at the interface. The area with too thick intermetallic compounds becomes the weak area of ​​the joint. In addition, this process does not mention an effective way to release the residual stress of the joint.

[0005] As an efficient solid-phase connection technology for homogeneous or heterogeneous metals, friction stir welding has the advantages of high efficiency, high quality, low welding stress and small deformation. However, in the actual operation process, a large amount of pressing must be introduced to ensure the performance of the joint, resulting in the joint thickness being significantly lower than the parent material thickness. In some application fields, the joint needs to be subjected to secondary machining, which increases the production process. In addition, friction stir welding usually requires a large axial force to ensure that sufficient friction heat is generated, which places certain requirements on the rigidity of the fixture.

[0006] The invention patent with application number CN 202011026042.4 discloses a method for achieving heterogeneous welding of aluminum alloy and titanium alloy. In order to avoid the generation of Ti / Al brittle phase in the welding zone, Sn is used as the welding transition metal. By stir friction welding, a high-quality friction welding weld is obtained. However, it should be pointed out that the problem that the thickness of the aluminum-titanium joint obtained by this process is lower than the thickness of the parent material has not been effectively solved. In some application operations, the joint still needs to be processed secondary.

[0007] It can be seen that under the condition of ensuring the thickness of heterogeneous metal welding joints, reducing the hazards of intermetallic compounds in heterogeneous metal welding joints (reducing thickness or changing shape), releasing the residual stress of the joints, and improving the strength of the welding joints, it is urgent to develop a low-cost, simple-to-operate and practical new process method to improve the performance of heterogeneous metal welding joints and provide technical support for high-performance connections of heterogeneous metals with large differences. Summary of the invention

[0008] In view of this, the present invention discloses a heterogeneous metal welding structure and a welding and riveting composite connection method using the same, and the specific scheme is as follows:

[0009] A heterogeneous metal welding structure comprises a metal plate A and a metal plate B. The welding joint between the metal plate A and the metal plate B is a butt joint. A prefabricated groove is provided on the upper surface of the metal plate A, and the prefabricated groove extends along the weld direction. A groove is provided on the metal plate B.

[0010] As a supplement to the technical solution of the present invention, the precast grooves are provided in one or more groups. When there are multiple groups of precast grooves, the multiple groups of precast grooves are parallel to each other and the distance between two adjacent groups of precast grooves is 1-2 mm.

[0011] As a supplement to the technical solution of the present invention, when a group of prefabricated grooves is provided, the prefabricated grooves are of dovetail groove structure.

[0012] As a supplement to the technical solution of the present invention, the angle of the groove formed on the metal plate B is 30°-40°.

[0013] The present invention also discloses a welding and riveting composite connection method using the above-mentioned heterogeneous metal welding structure, which is characterized by comprising the following steps:

[0014] A brazing welding gun is arranged above the prefabricated groove of metal plate A, and a stirring head of friction stir welding is arranged above the area between metal plate A and metal plate B. The welding gun is started, and the liquid metal after the welding wire is melted fills the prefabricated groove and then flows into the area between metal plate A and metal plate B to form filler metal. When the filler metal between metal plate A and metal plate B is in a semi-solid state, the stirring head of friction stir welding intervenes from the starting point of the area between metal plate A and metal plate B to complete the welding of metal plate A and metal plate B. During the welding process, the stirring head of friction stir welding moves in the same direction at the same speed as the welding gun. After the welding is completed, the welding gun is first turned off, and then the stirring head of friction stir welding is withdrawn, and the friction stir welding machine is turned off.

[0015] As a supplement to the technical solution of the present invention, TIG welding is used to fill the prefabricated groove, and the welding process parameters of TIG welding are specifically as follows: the distance between the tungsten electrode tip of the TIG welding gun and the horizontal plane of the stainless steel plate is 0.5-2.5mm, the argon shielding gas flow rate is 18-22L / min, the welding current is 20-200A, the welding speed is 1.5-4mm / s, and the wire feeding speed is 10-28mm / s.

[0016] As a supplement to the technical solution of the present invention, MIG welding is used to fill the prefabricated groove, and the welding process parameters of MIG welding are specifically as follows: the dry extension length of the MIG welding gun is set at 10-20mm, the argon shielding gas flow rate is 18-22L / min, the welding current is 20-200A, the welding speed is 1.5-4mm / s, and the wire feeding speed is 14-22mm / s.

[0017] As a supplement to the technical solution of the present invention, the specific welding process parameters of the friction stir welding are: rotation speed 400-1500r / min, shoulder pressure 0.1mm, welding speed 1.5-4mm / s, stirring needle inclination angle 2°-2.5°.

[0018] As a supplement to the technical solution of the present invention, the shoulder of the stir friction welding stirring head covers the prefabricated groove on the metal plate A and the groove on the metal plate B.

[0019] As a supplement to the technical solution of the present invention, the friction stir welding adopts static shoulder friction stir welding.

[0020] Beneficial effects:

[0021] 1. The present invention discloses a heterogeneous metal welding structure, which can realize the welding and riveting composite connection of two different metals and improve the strength of the welded joint.

[0022] 2. By opening the prefabricated groove on the metal plate A, the contact area between the metal plate A and the weld metal is increased, thereby increasing the joint strength. Brazing and friction stir welding are used in conjunction, so that the liquid metal formed after the welding wire is melted fills the prefabricated groove and then flows into the area between the two heterogeneous metal plates, forming a macroscopic welding and riveting composite connection.

[0023] 3. When the weld metal is in a semi-solid state, the friction stir treatment is used to break the brittle phases such as intermetallic compounds by large deformation, so as to reduce the thickness of the compound and refine the grain structure. In addition, the broken interface intermetallic compound layer exists in a serrated form, forming a microscopic welding and riveting composite connection in situ.

[0024] 4. After the friction stir welding process is introduced, the static shoulder of the stirring head reduces the peak temperature of the weld metal, improves the weld formation, and releases the residual stress inside the weld. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a structural schematic diagram of the present invention.

[0026] Figure 2 It is a schematic diagram of the side structure of metal plate A and metal plate B.

[0027] Figure 3 It is a schematic diagram of the side structure of metal plate A and metal plate B.

[0028] In the figure: 1. welding gun, 2. welding wire, 3. workbench, 4. stirring head, 5. welding direction, 6. metal plate A, 7. forming groove, 8. metal plate B, 9. prefabricated groove. DETAILED DESCRIPTION

[0029] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0030] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] like Figures 1 to 3 As shown, the present invention discloses a heterogeneous metal welding structure, which comprises a metal plate A and a metal plate B. The metal plate A and the metal plate B have different compositions. The welding joint of the metal plate A and the metal plate B is a butt joint. The upper surface of the metal plate A is provided with a prefabricated groove, which extends along the length direction of the weld. The metal plate B is provided with a groove. Preferably, the groove angle on the metal plate B is 30°-40°.

[0032] When two heterogeneous metal plates are welded by conventional fusion brazing, the residual stress near the weld joint area of ​​one of the metal plates after welding is large and the intermetallic compound is thick. Under this condition, it is necessary to open a prefabricated groove on the metal plate with large residual stress and thick intermetallic compound, and then use the welding structure disclosed in the present invention for welding. For example, if the residual stress near the weld joint area of ​​metal plate A is large and the metal compound is thick, it is necessary to open a prefabricated groove on metal plate A. The main reason for the above-mentioned large residual stress and thick intermetallic compound problems is that the chemical properties and thermophysical properties of heterogeneous metals are different.

[0033] In the present invention, fusion brazing is a welding method in which the interface of the high melting point side of the heterogeneous metal (such as steel, titanium, copper) is brazed, and the interface of the low melting point side (such as aluminum) is fusion welded. The welding method can be MIG, TIG, laser welding, or laser + TIG, laser + MIG or other welding methods, and is not limited to TIG welding or MIG welding disclosed in the present invention. Its main purpose is to melt the welding wire.

[0034] As a supplement to the technical solution of the present invention, the position where the prefabricated groove is opened is located near the edge of the area to be welded of the metal plate A. The prefabricated groove on the metal plate A is specifically a groove body opened on the upper surface of the metal plate A. The groove body can be intermittent or continuous, and is preferably continuous. The reason is that the use of a continuous groove body can increase the area of ​​the macro-welding and riveting composite connection and improve the overall strength of the welded joint.

[0035] As a supplement to the above technical solution, the precast grooves are provided in one or more groups. When there are multiple groups of precast grooves, the multiple groups of precast grooves are parallel to each other and the distance between two adjacent groups of precast grooves is 1-2 mm.

[0036] As a supplement to the above technical solution, the specific structure of the prefabricated groove can be any shape. When only one group of prefabricated grooves is provided, the prefabricated groove is preferably a dovetail groove structure. Preferably, the corners of the dovetail groove are rounded, so that the metal after the welding wire is melted can fully fill the prefabricated groove and prevent the generation of defects such as pores. Figure 2As shown in FIG. 1 , the corner position in the dovetail groove is set to a rounded structure so that the welding wire can fully fill the dovetail groove after melting. In addition, in order to ensure that the liquid metal after the welding wire melts fills the dovetail groove and can smoothly flow into the area between the metal plates A and B, as shown in FIG. Figure 2 As shown, the height of the upper end surface of the metal plate A located on the left side of the dovetail groove is higher than the height of the upper end surface of the metal plate A located on the right side of the dovetail groove.

[0037] As a preferred technical solution of the present invention, when the precast grooves are opened in three groups in total, the three groups of precast grooves are opened in relatively parallel, and the precast grooves can be straight or curved. When the precast grooves are curved structures, the contact area between the metal in the precast grooves and the metal in the weld area can be further increased, thereby increasing the strength of the welded joint.

[0038] like Figure 3 The three groups of prefabricated grooves are respectively prefabricated groove A, prefabricated groove B, and prefabricated groove C in terms of distance from the welding area from far to near, wherein the prefabricated groove A and the prefabricated groove C are both concave arc groove structures, and the prefabricated groove B is a dovetail groove structure. The spacing between two adjacent prefabricated grooves is 1-2 mm.

[0039] The present invention also discloses a welding and riveting composite connection method using the above-mentioned heterogeneous metal welding structure, which specifically comprises the following steps:

[0040] S1. Clean the plate to be welded by mechanical grinding to keep its surface flat and clean.

[0041] S2. Fix the metal plates A and B by a clamp. The welding joint is a butt joint. Use alcohol to wipe the groove on the metal plate B and the prefabricated groove on the surface of the metal plate A.

[0042] S3. A welding gun for brazing is arranged above the prefabricated groove area of ​​metal plate A, and a stirring head for friction stir welding is arranged above the area between metal plate A and metal plate B. The stirring head may cover the prefabricated groove on metal plate A or may not cover the prefabricated groove. Preferably, the shaft shoulder of the stirring head covers the prefabricated groove on metal plate A and the groove on metal plate B.

[0043] When the shoulder of the stirring head of the friction stir welding covers the prefabricated groove, during the friction stir welding process, the static shoulder on the stirring head compacts the metal in the prefabricated groove of the stainless steel plate to ensure that the prefabricated groove on the stainless steel plate is fully filled. At the same time, the stirring needle can release the stress of the metal in the prefabricated groove on the stainless steel plate to solve the problem of stress concentration. Secondly, during the processing of the weld joint, the stirring needle can make the metal flow, disperse it more evenly, achieve a dispersed distribution effect, break up the intermetallic compounds of the weld joint, and reduce the thickness of the intermetallic compounds.

[0044] During welding, the welding gun is first started to allow the welding wire to fill the prefabricated groove on the surface of the stainless steel plate. After the molten welding wire fills the prefabricated groove, the liquid metal flows into the area between the metal plate A and the metal plate B to form a filler metal. When the filler metal between the metal plate A and the metal plate B is in a semi-solid state, the stirring head of the friction stir welding intervenes from the starting point of the area between the metal plate A and the metal plate B to complete the welding of the metal plate A and the metal plate B. During the welding process, the stirring head of the friction stir welding moves in the same direction at the same speed as the welding gun.

[0045] The friction stir welding adopts static shoulder friction stir welding in which only the friction of the stirring needle generates heat to deform the material. The static shoulder friction stir welding is used to reduce the friction heat generated between the stirring head and the weld metal, reduce the peak temperature of the weld metal, improve the weld formation, and release the residual stress inside the weld.

[0046] The distance between the welding gun and the stirring head of the stir friction welding is 20-70mm, which can enable the liquid metal after the welding wire is melted to fill the prefabricated groove and then flow into the area between the metal plate A and the metal plate B. When the filler metal between A and the metal plate B is in a semi-solid state, stir friction welding at this time can reduce the damage of the stirring needle and improve the welding quality.

[0047] The semi-solid state specifically means that the weld metal is between solid and liquid, and contains part of the liquid phase, but the overall structure is still solid.

[0048] In the above welding process, when TIG welding is specifically selected for brazing, the welding process parameters are as follows: the distance between the tip of the welding gun and the horizontal plane of the titanium plate is 0.5-2.5mm, the argon shielding gas flow rate is 18-22L / min, the welding current is 20-200A, the welding speed is 1.5-4mm / s, and the wire feeding speed is 10-28mm / s, to ensure that the welding wire is fully melted and undergoes a metallurgical reaction with the base material.

[0049] In the above welding process, when MIG welding is specifically selected for brazing, the welding process parameters are as follows: the dry extension length of the MIG welding gun is set at 10-20mm, the argon shielding gas flow rate is 18-22L / min, the welding current is 20-200A, the welding speed is 1.5-4mm / s, and the wire feeding speed is 14-22mm / s.

[0050] The specific welding process parameters of stir friction welding are: rotation speed 400-1500r / min, shoulder pressure 0.1mm, welding speed 1.5-4mm / s, stirring needle inclination angle 2°-2.5°.

[0051] S4. After the welding is completed, the welding gun is first turned off, and then the stirring head of the friction stir welding is withdrawn and the friction stir welding machine is turned off.

[0052] The present invention adopts fusion brazing combined with stir friction welding to realize welding and riveting composite connection. Through the prefabricated groove of metal plate A, the molten welding wire and the molten liquid metal fill the prefabricated groove and then flow into the area between metal plate A and metal plate B. After welding, the metal in the prefabricated groove is connected with the metal in the weld area to form a macro welding and riveting composite connection, thereby improving the strength of the welded joint.

[0053] When the weld metal is in a semi-solid state, the friction stir treatment intervenes, using large deformation to break brittle phases such as intermetallic compounds, thereby reducing the compound thickness and refining the grain structure. In addition, the broken interface intermetallic compound layer exists in a serrated form, forming a microscopic weld-riveted composite connection in situ. After the friction stir treatment is intervened, the static shoulder of the stirring head reduces the peak temperature of A and the metal plate B, improves the weld formation, and releases the residual stress inside the weld.

[0054] In summary, the present invention innovatively proposes the use of a heterogeneous metal welding structure and a brazing-friction stir welding and riveting composite connection method to reduce the thickness of the intermetallic compound layer and change its morphology, thereby effectively releasing the residual stress of the joint; in addition, large deformation drives plastic flow to prompt the weld metal to fill the macro-mechanical prefabricated groove and form micro-interlocking in situ, ultimately achieving macro-micro mechanical bite and significantly improving the mechanical properties of the joint.

[0055] To facilitate the understanding of the technical solution, the present invention provides the following embodiments.

[0056] Embodiment 1:

[0057] Metal plate A is a stainless steel plate, and metal plate B is an aluminum alloy plate. The aluminum alloy plate is specifically a 5A06 grade aluminum alloy for welding, but is not limited to the above grades of aluminum alloys. The welding method disclosed in the present invention is also applicable to the welding of other grades of aluminum alloys and stainless steel. TIG welding is specifically used for brazing. The welding process specifically includes the following steps:

[0058] S1. Select 5A06 aluminum alloy plate and stainless steel plate of the same thickness, clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0059] S2. Fix the 5A06 aluminum alloy plate and the stainless steel plate by a clamp. The welding joint is a butt joint. To ensure sufficient metallurgical reaction on the aluminum alloy plate side, a 40° groove is opened on the 5A06 aluminum alloy plate, and a prefabricated groove of a dovetail groove structure is opened on the surface of the stainless steel plate. The groove on the 5A06 aluminum alloy plate and the prefabricated groove on the surface of the stainless steel plate are wiped with alcohol.

[0060] S3. A TIG welding gun is arranged above the prefabricated groove area of ​​the stainless steel plate, with the tungsten electrode tip of the TIG welding gun being 1 mm away from the horizontal plane of the steel plate; a stirring head for friction stir welding is arranged above the prefabricated groove and the area between the stainless steel plate and the aluminum alloy plate, with the shoulder of the stirring head covering the groove on the prefabricated groove and the aluminum alloy plate. The friction stir welding adopts static shoulder friction stir welding in which only the friction of the stirring needle generates heat to deform the material.

[0061] The distance between the TIG welding gun and the stirring head of the friction stir welding is 30mm. The liquid metal after the welding wire melts can fill the prefabricated groove and then flow into the area between the TC4 plate and the aluminum alloy plate to form filler metal. When the filler metal is in a semi-solid state, friction stir welding can reduce the damage of the stirring needle and improve the welding quality.

[0062] In the above welding process, the specific welding process parameters of TIG are: argon shielding gas flow rate 20L / min, welding current 90A, welding speed 2mm / s, and wire feeding speed 18mm / s.

[0063] The specific welding process parameters of friction stir welding are: rotation speed 900r / min, shoulder pressure 0.1mm, welding speed 2mm / s, and stirring needle inclination angle 2°.

[0064] S4. After welding is completed, first turn off the TIG welding gun, then withdraw the stirring head of the friction stir welding, and turn off the friction stir welding machine.

[0065] S5. The tensile strength of the aluminum-steel welded riveted joint was tested using a universal tensile testing machine, and the average strength of the aluminum-steel welded riveted joint was about 192 MPa.

[0066] Embodiment 2:

[0067] The metal plate A is a pure copper plate, and the metal plate B is an aluminum alloy plate. The aluminum alloy plate is specifically a 6061 grade aluminum alloy for welding, but is not limited to the above grade aluminum alloy. The welding method disclosed in the present invention is also applicable to the welding of other grades of aluminum alloys and stainless steel. The fusion brazing is specifically selected from MIG welding. The welding process specifically includes the following steps:

[0068] S1. Select 6061 aluminum alloy plates and pure copper plates of the same thickness, and clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0069] S2. Fix the 6061 aluminum alloy plate and the copper plate by a clamp. The welding joint is a butt joint. To ensure sufficient metallurgical reaction on the aluminum alloy plate side, a 40° groove is opened on the 6061 aluminum alloy plate, and a prefabricated groove of a dovetail groove structure is opened on the surface of the copper plate. The groove on the 6061 aluminum alloy plate and the prefabricated groove on the surface of the copper plate are wiped with alcohol.

[0070] S3. A MIG welding gun is arranged above the prefabricated groove area of ​​the copper plate, the dry extension length is set to 12 mm, and a stirring head for stir friction welding is arranged above the prefabricated groove and the area between the copper plate and the aluminum alloy plate.

[0071] The distance between the MIG welding gun and the stirring head of the friction stir welding is 25mm, which can enable the liquid metal after the welding wire is melted to fill the prefabricated groove and then flow into the area between the copper plate and the aluminum alloy plate. When the weld metal is in a semi-solid state, friction stir welding can reduce the damage of the stirring needle and improve the welding quality.

[0072] In the above welding process, the welding process parameters of MIG welding are specifically: argon shielding gas flow rate 20L / min, welding current 70A, welding speed 1.5mm / s, and wire feeding speed 14mm / s.

[0073] The specific welding process parameters of friction stir welding are: rotation speed 700r / min, shoulder pressure 0.1mm, welding speed 1.5mm / s, and stirring needle inclination angle 2°.

[0074] S4. After welding is completed, first turn off the MIG welding gun, then withdraw the stirring head of the friction stir welding, and turn off the friction stir welding machine.

[0075] The tensile strength of the aluminum-copper welded rivet joints was tested using a universal tensile testing machine, and the average strength of the aluminum-copper welded rivet joints obtained was about 172 MPa.

[0076] Embodiment 3:

[0077] The metal plate A is a TC4 titanium alloy plate, and the metal plate B is an aluminum alloy plate. The aluminum alloy plate is specifically a 5A06 grade aluminum alloy for welding, but is not limited to the above grades of aluminum alloys. The welding method disclosed in the present invention is also applicable to the welding of other grades of aluminum alloys and stainless steel. The fusion brazing is specifically TIG welding. The welding process specifically includes the following steps:

[0078] S1. Select 5A06 aluminum alloy plates and TC4 plates of the same thickness, and clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0079] S2. The 5A06 aluminum alloy plate and the TC4 plate are fixed by a clamp. The welding joint is a butt joint. To ensure sufficient metallurgical reaction on the aluminum alloy plate side, a 40° groove is opened on the 5A06 aluminum alloy plate, and three sections of prefabricated grooves are opened on the plate surface. From left to right, the spacing of each section is 2mm and 1mm respectively. The groove on the 5A06 aluminum alloy plate and the prefabricated groove on the surface of the TC4 plate are wiped with alcohol.

[0080] S3. A TIG welding gun is arranged above the prefabricated groove area of ​​the plate, so that the distance between the tungsten tip of the TIG welding gun and the horizontal plane of the TC4 plate is 1 mm, and a stirring head for stir friction welding is arranged above the prefabricated groove and the area between the TC4 plate and the aluminum alloy plate.

[0081] The distance between the TIG welding gun and the stirring head of the stir friction welding is 25mm, which can enable the liquid metal after the welding wire is melted to fill the prefabricated groove and then flow into the area between the TC4 plate and the aluminum alloy plate. When the weld metal is in a semi-solid state, stir friction welding can reduce the damage of the stirring needle and improve the welding quality.

[0082] In the above welding process, the specific welding process parameters of TIG are: argon shielding gas flow rate 20L / min, welding current 80A, welding speed 2mm / s, and wire feeding speed 10mm / s.

[0083] The specific welding process parameters of friction stir welding are: rotation speed 700r / min, shoulder pressure 0.1mm, welding speed 2mm / s, and stirring needle inclination angle 2°.

[0084] S4. After welding is completed, first turn off the TIG welding gun, then withdraw the stirring head of the friction stir welding, and turn off the friction stir welding machine.

[0085] The tensile strength of the aluminum-titanium welded rivet joints was tested using a universal tensile testing machine, and the average strength of the aluminum-titanium welded rivet joints obtained was about 236 MPa.

[0086] Comparative Example 1:

[0087] S1. Select 5A06 aluminum alloy plate and stainless steel plate of the same thickness, clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0088] S2. Fix the 5A06 plate and the stainless steel plate with a clamp. The welding joint is a butt joint. A 40° groove is opened on the 5A06 plate and the stainless steel. The grooves on the 5A06 plate and the stainless steel are wiped with alcohol.

[0089] S3. Set the TIG welding gun just above the gap between the stainless steel plate and the 5A06 plate, with the distance between the tungsten tip of the TIG welding gun and the horizontal plane of the steel plate being 1 mm;

[0090] S4. During the formal welding, the TIG welding gun is started to fill the groove of the aluminum alloy plate and the stainless steel plate with welding wire. The welding process parameters of TIG welding are the same as those in Example 1.

[0091] S5. Welding is finished and the TIG welding gun is turned off.

[0092] The tensile strength of aluminum-steel brazing joints was tested using a universal tensile testing machine. The average strength of the aluminum-steel brazing joints was about 115 MPa.

[0093] By comparing Implementation 1 with Comparative Example 1, the aluminum-steel joint was prepared by the brazing-friction stir welding and riveting composite connection method of the present invention, and the tensile strength of the joint was increased by about 70%.

[0094] Comparative Example 2:

[0095] S1. Select 6061 aluminum alloy plates and copper plates of the same thickness, and clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0096] S2. Fix the 6061 plate and the copper plate by a clamp, the welding joint is a butt joint, a 40° groove is opened on the 6061 plate and the copper, and the grooves on the 6061 plate and the copper are wiped with alcohol;

[0097] S3. Set the MIG welding gun just above the gap between the copper plate and the 6061 plate, and set the dry extension length to 12mm;

[0098] S4. During the formal welding, the MIG welding gun is started to fill the groove of the aluminum alloy plate and the copper plate with welding wire. The welding process parameters of the MIG welding are the same as those in Example 2.

[0099] S5. Welding is finished and the MIG welding gun is turned off.

[0100] The tensile strength of the aluminum-copper brazing joint was tested using a universal tensile testing machine. The average strength of the aluminum-copper brazing joint was about 111 MPa.

[0101] By comparing Example 2 with Comparative Example 2, the aluminum-copper joint was prepared by the brazing-friction stir welding and riveting composite connection method of the present invention, and the tensile strength of the joint was increased by about 55%.

[0102] Comparative Example 3:

[0103] S1. Select 5A06 aluminum alloy plates and TC4 plates of the same thickness, and clean the plates by mechanical grinding to keep their surfaces flat and clean.

[0104] S2. Fix the 5A06 plate and TC4 plate by a fixture. The welding joint is a butt joint. A 40° groove is opened on both the 5A06 plate and TC4. The grooves on the 5A06 plate and TC4 are wiped with alcohol.

[0105] S3. Set a TIG welding gun just above the gap between the TC4 plate and the 5A06 plate, with the distance between the tungsten electrode tip of the TIG welding gun and the horizontal plane of the titanium plate being 1 mm;

[0106] S4. During the formal welding, the TIG welding gun is started to fill the groove of the aluminum alloy plate and the TC4 plate with welding wire. The welding process parameters of TIG welding are the same as those in Example 3.

[0107] S5. Welding is finished and the TIG welding gun is turned off.

[0108] The tensile strength of the aluminum-titanium fusion brazing welded joint was tested with a universal tensile testing machine, and the average strength of the aluminum-titanium fusion brazing welded joint was about 127 MPa. Comparing Example 3 with Comparative Example 3, the tensile strength of the aluminum-titanium joint prepared by the fusion brazing-friction stir welding and riveting composite connection method of the present invention was increased by about 86%.

[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Heterogeneous metal welding structure, characterized in that: The invention comprises a metal plate A and a metal plate B, wherein the welding joint of the metal plate A and the metal plate B is a butt joint, wherein the upper surface of the metal plate A is provided with a prefabricated groove, the prefabricated groove extends along the direction of the weld, and the metal plate B is provided with a groove, and the prefabricated groove on the upper surface of the metal plate A and the groove on the metal plate B are covered by the shoulder of the friction stir welding stirring head; The prefabricated groove on the upper surface of the metal plate A and the area between the metal plate A and the metal plate B are used to fill the liquid metal after the welding wire of the brazing is melted to form the filler metal, and the filler metal is in a semi-solid state. The stirring head of the stir friction welding intervenes from the starting point of the area between the metal plate A and the metal plate B to complete the welding of the metal plate A and the metal plate B; The brazing is TIG welding or MIG welding. When the brazing is TIG welding, the welding process parameters of TIG welding are as follows: the distance between the tungsten tip of the TIG welding gun and the horizontal plane of the metal plate A is 0.5-2.5 mm, the flow rate of argon shielding gas is 18-22 L / min, the welding current is 20-200 A, the welding speed is 1.5-4 mm / s, and the wire feeding speed is 10-28 mm / s; When the fusion brazing is MIG welding, the specific welding process parameters of MIG welding are: the dry extension length of the MIG welding gun is set at 10-20 mm, the argon shielding gas flow rate is 18-22 L / min, the welding current is 20-200 A, the welding speed is 1.5-4 mm / s, and the wire feeding speed is 14-22 mm / s; The specific welding process parameters of friction stir welding are: rotation speed 400-1500 r / min, shoulder pressure 0.1 mm, welding speed 1.5-4 mm / s, and stirring needle inclination angle 2°-2.5°.

2. The heterogeneous metal welding structure according to claim 1, characterized in that: The precast grooves are provided in one or more groups. When there are multiple groups of precast grooves, the multiple groups of precast grooves are parallel to each other and the distance between two adjacent groups of precast grooves is 1-2 mm.

3. The heterogeneous metal welding structure according to claim 2, characterized in that: When a group of prefabricated grooves is provided, the prefabricated grooves are dovetail groove structures.

4. The heterogeneous metal welding structure according to claim 1, characterized in that: The angle of the groove of the metal plate B is 30°-40°.

5. A welding and riveting composite connection method for heterogeneous metal welding structures according to any one of claims 1 to 4, characterized in that: The following steps are involved: A welding gun for brazing is arranged above the prefabricated groove of metal plate A, and a stirring head for friction stir welding is arranged above the area between metal plate A and metal plate B. The welding gun is started, and the liquid metal after the welding wire melts fills the prefabricated groove and then flows into the area between metal plate A and metal plate B to form filler metal. When the filler metal between metal plate A and metal plate B is in a semi-solid state, the stirring head for friction stir welding intervenes from the starting point of the area between metal plate A and metal plate B to complete the welding of metal plate A and metal plate B. During the welding process, the stirring head for friction stir welding and the welding gun move in the same direction at the same speed. After welding is completed, the welding gun is first turned off, and then the stirring head of the friction stir welding is withdrawn and the friction stir welding machine is turned off.

6. The welding and riveting composite connection method of heterogeneous metal welding structures according to claim 5 is characterized in that: The shoulder of the friction stir welding stirring head covers the prefabricated groove on the metal plate A and the groove on the metal plate B.

7. The welding and riveting composite connection method of heterogeneous metal welding structures according to claim 5 is characterized in that: The friction stir welding adopts static shoulder friction stir welding.

Citation Information

Patent Citations

  • Method for implementing heterogeneous welding of titanium alloy and aluminum alloy

    CN112207419A

  • Laser welding method of titanium alloy plate

    CN106735906A

  • Fusion welding auxiliary heating friction-stir welding method under prefabricated groove situation

    CN108857114A

  • Dissimilar metal electric arc melting-brazing method based on biting assistance

    CN111151904A

  • Method for improving strength of steel-aluminum dissimilar welded joint through mechanical and metallurgical dual combination

    CN113118599A