A Cu-doped SnO thin film transistor, complementary logic circuit and preparation method thereof

Through copper-doped SnO thin film transistor technology, the problems of low carrier mobility of SnO thin film transistors and difficulty in turning off inverter devices are solved, and high-performance n-type and p-channel Cu-doped SnO thin film transistors and complementary type logic circuit, suitable for flexible electronic products.

CN117976544BActive Publication Date: 2024-10-01RISEN SEMICON TECH (HUNAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410013921.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-10-01
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

In the existing technology, SnO thin film transistors have low carrier mobility, and SnO-based inverter devices are difficult to completely turn off, hindering their application in complementary logic circuits, especially in flexible electronic products.

Method used

Using copper (Cu) doped SnO thin film transistors, an n-channel Cu doped SnO thin film transistor is obtained by depositing a Cu:Sn film and annealing it after encapsulating the hafnium oxide layer, and performs plasma treatment in an argon environment. By controlling the threshold voltage, a p-channel Cu-doped SnO thin film transistor and a complementary logic circuit based on p-type and n-type channels were prepared.

Benefits of technology

Significantly improve the electron mobility of n-channel Cu-doped SnO thin film transistors and the hole mobility of p-channel Cu-doped SnO thin film transistors, achieve high current switching ratio and ultra-high voltage gain, and achieve high current switching ratio and ultra-high voltage gain on flexible linings. On the bottom, the stability and bending reliability of complementary logic circuits have been successfully achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117976544B_ABST
    Figure CN117976544B_ABST
Patent Text Reader

Abstract

The present invention provides a copper-doped tin oxide (Cu:SnO) thin film transistor, a complementary logic circuit and a preparation method thereof, and belongs to the field of semiconductor technology. The device comprises a substrate, a back gate electrode layer, a gate dielectric layer, a semiconductor channel material, an electrode layer and a hafnium oxide layer stacked in sequence. The present invention obtains p-type and / or n-type channel Cu:SnO thin film transistors through different annealing sequences, uses plasma treatment technology to regulate the threshold voltage of the p-type channel Cu:SnO, and successfully prepares a complementary logic circuit on this basis. The proposed integration technology successfully breaks through the application of a single metal oxide in complementary logic circuits, and is applied to flexible substrates, providing new ideas and technologies for future applications in the field of flexible electronics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a Cu-doped SnO thin film transistor, a complementary logic circuit and a preparation method thereof. Background Art

[0002] Complementary metal-oxide-semiconductor logic circuits have the advantages of low power consumption, wide noise margin, and mass production, which have promoted the rapid development of the integrated circuit industry.

[0003] However, conventional silicon-based complementary metal-oxide-semiconductor logic circuits face problems of rigidity and brittleness, which hinder their application in emerging flexible electronics (wearable devices, artificial skin, flexible displays, etc.). Metal oxide semiconductors show great commercial application potential in flexible electronics due to their high carrier mobility and low-temperature deposition process on plastic substrates. For example, amorphous IGZO has been commercialized in flexible displays, and p-type Cu-based 2 Complementary logic of O and n-type IGZO, ZTO, etc. has been demonstrated. However, due to the incompatibility of processing technology between various metal oxide semiconductors, this may lead to complex layout and high cost of production in the circuit, hindering the commercial application of this process.

[0004] In the study of various metal oxide semiconductors, SnO has been proved to be the only metal oxide semiconductor that can transport conductive electrons and holes due to the influence of Sn's 5p orbital on the bottom of the conduction band and the 5s orbital on the top of the valence band. Although bipolar SnO thin film transistors show application potential in complementary logic circuits, the carrier mobility of bipolar devices is low. In addition, the inverter integrating n-channel and p-channel thin film transistors has a clear on / off state, and the inverter based on SnO thin film transistors is difficult to be completely turned off.

[0005] Therefore, it is urgent to develop an effective strategy to improve the performance of n- and p-channel SnO devices. The top of the valence band of SnO comes from the hybridization of the O 2p orbital and the Sn 5s orbital, and the spherical expansion of the Sn 5s orbital gives SnO a high hole mobility. At the same time, the bottom of the conduction band is mainly composed of the Sn 5p orbital, and the partial state density curve presents a free electron band, which is conducive to electron transport. In addition, since the direct (optical) band gap of SnO is 2.7eV and the indirect (basic) band gap is 0.7eV, it has a small ionization potential and a large electron affinity, and can be p- and n-type doped.

[0006] Currently, it is extremely important to explore effective doping elements and processing techniques to realize p-channel and n-channel SnO thin film transistors. It is a major challenge that needs to be solved urgently to realize the preparation of complementary logic devices using a single metal oxide semiconductor, and it is of great significance to the development of complementary logic circuits. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a tin oxide (SnO) thin film transistor based on copper (Cu) doping, a complementary logic circuit and a preparation method thereof, and specifically provide an n-type channel Cu-doped SnO thin film transistor, a p-type channel Cu-doped SnO thin film transistor, a SnO complementary logic circuit based on p-type and n-type channel Cu doping and a preparation method thereof.

[0008] In a first aspect, the present invention provides a method for preparing an n-type channel Cu-doped SnO thin film transistor, the method comprising:

[0009] Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer;

[0010] Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer to obtain a Cu:Sn film;

[0011] Step three, depositing an electrode layer on the surface of the Cu:Sn film;

[0012] Step 4, growing a hafnium oxide layer on the surface of the device obtained in step 3;

[0013] Step five: annealing to obtain an n-type channel Cu-doped SnO thin film transistor.

[0014] In a second aspect, the present invention provides an n-type channel Cu-doped SnO thin film transistor, wherein the n-type channel Cu-doped SnO thin film transistor comprises a substrate, a back gate electrode layer, a gate dielectric layer, a semiconductor channel material, an electrode layer and a hafnium oxide layer stacked in sequence, wherein the semiconductor channel material is Cu-doped SnO, and the semiconductor channel material is obtained by annealing a Cu:Sn thin film after encapsulating the hafnium oxide layer.

[0015] In a third aspect, the present invention provides a method for preparing a p-type channel Cu-doped SnO thin film transistor, the method comprising:

[0016] Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer;

[0017] Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer to obtain a Cu:Sn film;

[0018] Step 3: annealing to obtain a p-type Cu-doped SnO channel material;

[0019] Step 4, depositing an electrode layer on the surface of the p-type Cu-doped SnO channel material to obtain a thin film transistor;

[0020] Step 5, growing a hafnium oxide layer on the surface of the thin film transistor to obtain a p-type channel Cu-doped SnO thin film transistor;

[0021] Step six, using a plasma cleaning machine to perform plasma treatment on the p-type channel Cu-doped SnO thin film transistor obtained in step five in an argon environment, so as to achieve regulation of the threshold voltage.

[0022] In a fourth aspect, the present invention provides a p-type channel Cu-doped SnO thin film transistor, wherein the p-type channel Cu-doped SnO thin film transistor comprises a substrate, a back gate electrode layer, a gate dielectric layer, a semiconductor channel material, an electrode layer and a hafnium oxide layer stacked in sequence, wherein the semiconductor channel material is Cu-doped SnO.

[0023] In a fifth aspect, the present invention provides a method for preparing a SnO complementary logic circuit based on p-type and n-type channel Cu doping, the method comprising:

[0024] Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer;

[0025] Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer, and obtaining a p-type Cu:SnO channel material after annealing;

[0026] Step 3, depositing a Cu-doped metal Sn film next to the p-type Cu:SnO channel material;

[0027] Step 4, depositing an electrode layer on the surface of the device after completing step 3 to obtain a p-type channel Cu:SnO thin film transistor;

[0028] Step 5, growing a hafnium oxide layer on the surface of the device in step 4;

[0029] Step six, annealing to obtain n-type channel Cu-doped SnO channel material, and obtain SnO complementary logic circuit based on p-type and n-type channel Cu-doping;

[0030] Step seven: using a plasma cleaning machine to perform plasma treatment on the complementary logic circuit in an argon environment to achieve regulation of the threshold voltage.

[0031] In a sixth aspect, the present invention provides a complementary logic circuit based on p-type and n-type channel Cu-doped SnO, the complementary logic circuit comprising a substrate, a back gate electrode layer, a gate dielectric layer, a semiconductor channel material, an electrode layer and a hafnium oxide layer stacked in sequence, the semiconductor channel material being Cu-doped SnO, including a p-type Cu:SnO channel material and an n-type Cu:SnO channel material.

[0032] In general, compared with the prior art, the technical solution conceived by the present invention can achieve the following beneficial effects:

[0033] 1. In hafnium oxide (HfO 2 ) After packaging, the Cu 3at% :Sn film was annealed to obtain n-type channel Cu 3at% :SnO thin film transistor. Due to the strong reducing property of Hf atoms, O atoms near the Sn vacancies migrate to the hafnium oxide layer, which suppresses the p-type conductivity in SnO. In addition, Cu 1+ It can induce the formation of n-type doping effect and suppress electron-electron scattering by eliminating the degeneracy of conduction band energy level. 3at% The electron mobility of SnO thin film transistors reaches 43cm 2 V -1 s -1 Above, the current switching ratio reaches 6.8×10 4 above.

[0034] 2. Directly on Cu 3at% :Sn thin film can be annealed to obtain p-type channel Cu 3at% :SnO thin film transistor, and then grow a hafnium oxide layer on the surface of the transistor. By plasma treating the device in an argon environment, Hf can be migrated to the Cu:SnO thin film, so that the threshold voltage of the device moves in the negative direction, and an enhanced p-type channel Cu is obtained. 3at% SnO thin film transistor, its hole mobility reaches 2cm 2 V -1 s -1 Above, the current switching ratio reaches 1.3×10 4 above.

[0035] 3. In n-type and p-type channel Cu 3at% : On the basis of SnO thin film transistors, a complementary logic circuit based on p-type and n-type channel Cu-doped SnO was successfully prepared. The logic circuit prepared by the present invention has an ultra-high voltage gain of more than 302, as well as excellent working stability and bending reliability, and successfully realizes a complementary logic circuit based on a metal oxide semiconductor on a flexible substrate.

[0036] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and the drawings.

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 A schematic diagram of the structure of an n-type channel Cu:SnO thin film transistor prepared in Example 1 of the present invention;

[0040] Figure 2 A relationship diagram between source-drain current and gate voltage measured at different Cu doping concentrations at a source-drain voltage of -1V for an n-type channel Cu:SnO thin film transistor prepared in Example 1 of the present invention and a comparative example;

[0041] Figure 3 A schematic diagram of the structure of a p-type channel Cu:SnO thin film transistor prepared in Example 2 of the present invention;

[0042] Figure 4 A p-type channel Cu prepared in Example 2 of the present invention 3at% : The relationship between the source-drain current and the gate voltage of the SnO thin film transistor measured after plasma treatment in an argon environment for different times when the source-drain voltage is -1V;

[0043] Figure 5 A Cu based on p-type and n-type channel provided in the third embodiment of the present invention 3at% : Schematic diagram of the structure of SnO complementary logic circuit;

[0044] Figure 6 A Cu based on p-type and n-type channel provided in the third embodiment of the present invention 3at% : Flow chart of the preparation method of SnO complementary logic circuit;

[0045] Figure 7 A relationship diagram between the output voltage and input voltage of a device measured at different driving voltages based on a p-type and n-type channel complementary logic circuit provided in the third embodiment of the present invention;

[0046] Figure 8 A Cu based on p-type and n-type channel provided in the third embodiment of the present invention 3at%: The relationship between the voltage gain and input voltage of the device measured at different driving voltages of the SnO complementary logic circuit;

[0047] Fig. 9 A Cu based on p-type and n-type channel provided in the third embodiment of the present invention 3at% : Performance diagram of the SnO complementary logic circuit in terms of device working stability and bending reliability test when the driving voltage is 50V.

[0048] Among them, the figure markings are: 1—substrate, 2—back gate electrode layer, 3—gate dielectric layer, 4—Cu:SnO channel material, 4a—p-type Cu:SnO channel material, 4b—n-type Cu:SnO channel material, 5a—source electrode, 5b—drain electrode, 5c—output electrode, 6—hafnium oxide layer. DETAILED DESCRIPTION

[0049] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, so that the above-mentioned and other objects, features and advantages of the present invention will be clearer. The same figure marks in all the drawings indicate the same parts. The drawings are not deliberately drawn to scale, and the focus is on illustrating the main purpose of the present invention. The described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0050] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0051] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0052] Embodiment 1

[0053] A method for preparing an n-type channel Cu-doped SnO (Cu:SnO) thin film transistor is provided in Example 1 of the present invention. Figure 1 , Figure 1 The schematic diagram of the structure of an n-type channel Cu:SnO thin film transistor prepared in Example 1 of the present invention is shown in FIG. 1 . The preparation method provided in Example 1 specifically includes the following steps:

[0054] Step 1: fabricate a substrate 1, a back gate electrode layer 2, and a gate dielectric layer 3 in sequence.

[0055] Preferably, the substrate 1 is a flexible substrate.

[0056] In the embodiment of the present invention, step one specifically includes:

[0057] S11: PI (polyimide) is selected as the flexible substrate 1, and the PI substrate is deposited on a clean glass carrier by spin coating until the device is completed and then separated.

[0058] S12: Depositing an aluminum electrode layer directly on the PI substrate 1 as a back gate electrode layer 2 by sputtering.

[0059] S13: Anodize a layer of Al on the surface of the back gate electrode layer 2 2 O 3 As the gate dielectric layer 3.

[0060] Preferably, the thickness of the PI flexible substrate 1 layer is 18 μm, the thickness of the back gate electrode layer 2 is 170 nm, and the thickness of the gate dielectric layer 3 is 200 nm.

[0061] Step 2: depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer to obtain a Cu:Sn film.

[0062] Specifically, a Cu-doped metal Sn film (Cu:Sn film) is deposited using a metal mask and a magnetron sputtering coating system.

[0063] Preferably, the Cu:Sn film partially covers the surface of the gate dielectric layer 3 .

[0064] In this embodiment, the Cu:Sn thin film is obtained by sintering and fusing metal Cu and Sn to form a target material, and then depositing it through a magnetron sputtering coating system.

[0065] Step three, using a metal mask and a thermal evaporation coating system to deposit an electrode layer on the surface of the Cu:Sn film.

[0066] Specifically, the upper and lower electrodes are deposited on the surface of the Cu:Sn film by using a metal mask and a thermal evaporation coating system, and the evaporation rate is The upper electrode is made of gold (Au) with a thickness of 40-70nm, while the lower electrode is made of chromium (Cr) with a thickness of 10-15nm. The lower electrode contacts the channel material. This structure can ensure the formation of good ohmic contact.

[0067] Preferably, the electrode layer comprises a source electrode 5a and a drain electrode 5b, and the source electrode 5a and the drain electrode 5b have no physical contact.

[0068] Step 4, using an atomic layer deposition system to grow a hafnium oxide layer 6 on the surface of the device obtained in step 3;

[0069] In this embodiment, step four specifically includes: keeping the tetrakis(dimethylamino)hafnium precursor at 75°C, keeping the water precursor at room temperature, using high-purity nitrogen as a carrier and protective gas, and transporting the tetrakis(dimethylamino)hafnium precursor and the water precursor to a reaction chamber with a temperature of 100°C for reaction.

[0070] In this embodiment, the atomic layer deposition process of the hafnium oxide layer 6 is performed for a total of 80 cycles, wherein the thickness of one growth cycle is Thus, a hafnium oxide layer 6 having a thickness of 9.6 nm was obtained.

[0071] Among them, a growth cycle includes: first, high-purity nitrogen gas continuously transports tetrakis(dimethylamino)hafnium precursor to the reaction chamber for 100s-120s, and then stops transporting the tetrakis(dimethylamino)hafnium precursor; then, high-purity nitrogen gas continuously transports water precursor to the reaction chamber for 100s-120s, and then stops transporting the water precursor.

[0072] Step five: annealing to obtain an n-type channel Cu-doped SnO (Cu:SnO) thin film transistor.

[0073] In this embodiment, step five specifically includes annealing at 250° C. for 10 min in an air environment using a tube furnace to obtain an n-type Cu:SnO channel material 4 to obtain an n-type channel Cu:SnO thin film transistor.

[0074] The hafnium oxide layer 6 at least partially contacts the electrode layer and / or the Cu:SnO channel material 4 .

[0075] The present invention performs a performance test on the n-type channel Cu:SnO thin film transistor prepared in Example 1 and a comparative example of a SnO thin film transistor without Cu doping. Figure 2 , Figure 2 The relationship between the source-drain current and the gate voltage of the n-type channel Cu:SnO thin film transistors doped with different contents of Cu prepared in the embodiment of the present invention and the comparative example of the thin film transistor without Cu doping is -1V. It can be seen that when the doping atomic ratio of Cu is 3%, the transfer characteristic curve of the device shows good n-type characteristics. The test shows that the n-channel Cu 3at% The electron mobility of SnO thin film transistors reaches 43.8 cm 2 V -1 s -1 , the current switching ratio is 6.8×10 4 Compared with non-Cu-doped SnO thin film transistors, the mobility and switching ratio are improved by 1-2 orders of magnitude.

[0076] This embodiment only provides a demonstration of the present invention, and its specific parameters are not limited by the embodiment, such as the substrate material, electrode material, material thickness, specific parameters, etc. are not limited by the embodiment.

[0077] Embodiment 2

[0078] A second embodiment of the present invention provides a method for preparing a p-type channel Cu-doped SnO (Cu:SnO) thin film transistor.

[0079] This embodiment focuses on the differences from the first embodiment, and the similarities are not repeated here.

[0080] See also Figure 3 , Figure 3 A schematic structural diagram of a p-type channel Cu:SnO thin film transistor prepared by the preparation method provided in Example 2 of the present invention.

[0081] Step 1: manufacturing a substrate 1, a back gate electrode layer 2, and a gate dielectric layer 3.

[0082] The specific process is shown in Example 1.

[0083] Step 2: fabricating a p-type Cu:SnO channel material 4 on the surface of the gate dielectric layer 3 .

[0084] Specifically, a Cu-doped metal Sn film is deposited using a metal mask and a magnetron sputtering coating system to obtain a Cu:Sn film, and a p-type Cu:SnO channel material 4 is obtained by annealing in air at 250° C. for 10 minutes using a tube furnace.

[0085] Step three: deposit an electrode layer on the surface of the p-type Cu:SnO channel material 4 using a metal mask and a thermal evaporation coating system to obtain a p-type channel Cu-doped SnO thin film transistor.

[0086] The specific process is shown in Example 1.

[0087] Step 4: grow a hafnium oxide layer 6 on the surface of the thin film transistor using an atomic layer deposition system to obtain a p-type channel Cu-doped SnO thin film transistor.

[0088] The specific process is shown in Example 1.

[0089] The hafnium oxide layer 6 at least partially contacts the electrode layer and / or the Cu:SnO channel material 4 .

[0090] Step 5: Perform plasma treatment on the p-type channel Cu:SnO thin film transistor obtained in step 4 in an argon environment using a plasma cleaning machine to achieve regulation of the threshold voltage.

[0091] Specifically, the device was treated for 180 seconds using a plasma cleaner in an argon environment at a power of 100 watts.

[0092] In this embodiment, the plasma treatment can make hafnium (Hf) migrate to the p-type Cu:SnO channel material, so that the threshold voltage of the device moves in the negative direction, and an enhanced p-type channel Cu is obtained. 3at% :SnO thin film transistor to achieve threshold voltage regulation.

[0093] The present invention has carried out performance tests on the p-type channel Cu:SnO thin film transistor prepared in this embodiment and the initial comparative example without hafnium oxide layer, see Figure 4 , Figure 4 A p-type channel Cu prepared in Example 2 of the present invention 3at% : When the source-drain voltage of SnO thin film transistor is -1V, the source-drain current and gate voltage measured at different plasma treatment times, as well as the source-drain current and gate voltage measured in the initial comparative example without hafnium oxide layer. It can be seen from the figure that plasma treatment can move the threshold voltage of the device to the negative direction, obtaining an enhanced p-type channel Cu 3at% :SnO thin film transistor, its hole mobility reaches 2.4cm 2 V -1 s -1 , the current switching ratio reaches 1.3×10 4 Compared with the non-Cu-doped SnO thin film transistor, the mobility and switching ratio have good performance.

[0094] This embodiment only provides a demonstration of the present invention, and its specific parameters are not limited by the embodiment, such as the substrate material, electrode material, material thickness, specific parameters, etc. are not limited by the embodiment.

[0095] Embodiment 3

[0096] A method for preparing a p-type and n-type channel Cu:SnO complementary logic circuit is provided in the third embodiment of the present invention. Figure 5 and Figure 6 , specifically including the following steps:

[0097] Step 1: fabricate a substrate 1, a back gate electrode layer 2, and a gate dielectric layer 3.

[0098] The specific process is shown in Example 1.

[0099] Step 2: preparing a p-type Cu:SnO channel material 4 a on the surface of the gate dielectric layer 3 .

[0100] In this embodiment, a Cu:Sn thin film is deposited using a metal mask and a magnetron sputtering coating system, and annealed at 250° C. for 10 min in an air environment using a tube furnace to obtain a p-type Cu:SnO channel material 4 a .

[0101] Step three: deposit a Cu:Sn thin film next to the p-type Cu:SnO channel material 4a using a metal mask and a magnetron sputtering coating system.

[0102] The Cu:Sn film and the p-type Cu:SnO channel material 4a do not need to be in direct physical contact.

[0103] Step 4: using a metal mask and a thermal evaporation coating system to deposit an electrode layer on the surface of the device after step 3, to obtain a p-type channel Cu:SnO thin film transistor;

[0104] The specific process is shown in Example 1.

[0105] Preferably, the electrode layer includes a source electrode 5a, a drain electrode 5b and an output electrode 5c, and the source electrode 5a, the drain electrode 5b and the output electrode 5c have no physical contact.

[0106] Step 5: Using an atomic layer deposition system to grow hafnium oxide (HfO 2 ) layer 6.

[0107] The specific process is shown in Example 1.

[0108] Step six, annealing, obtaining n-type Cu:SnO channel material 4b next to p-type Cu:SnO channel material 4a, and obtaining a complementary logic circuit based on p-type and n-type channel Cu-doped SnO.

[0109] Specifically, annealing was performed in air at 250° C. for 10 min using a tube furnace to obtain an n-type Cu:SnO channel material 4b next to the p-type Cu:SnO channel material 4a;

[0110] Preferably, the hafnium oxide layer 6 at least partially contacts the electrode and / or the Cu:SnO channel material.

[0111] Step seven: using a plasma cleaning machine to perform plasma treatment on the complementary logic circuit in an argon environment to achieve regulation of the threshold voltage.

[0112] Plasma treatment can make Hf migrate into the Cu:SnO film, causing the threshold voltage of the device to move negatively, and obtaining an enhanced p-type channel Cu 3at% :SnO thin film transistor to achieve threshold voltage regulation.

[0113] This embodiment only provides a demonstration of the present invention, and its specific parameters are not limited by the embodiment, such as the substrate material, electrode material, material thickness, specific parameters, etc. are not limited by the embodiment.

[0114] The present invention performs a performance test on the complementary logic circuit based on SnO doped with p-type and n-type channels obtained by the preparation method of the third embodiment. Figures 7 to 9 The performance test results of the complementary logic circuit based on p-type and n-type channel Cu-doped SnO are shown.

[0115] in, Figure 7 A diagram showing the relationship between the output voltage and input voltage of a device of a complementary logic circuit based on p-type and n-type channel Cu-doped SnO under different driving voltages provided by an embodiment of the present invention. The experimental results show that the logic circuit exhibits good voltage conversion characteristics.

[0116] Figure 8 A diagram showing the relationship between the voltage gain and input voltage of a device measured at different driving voltages for a complementary logic circuit based on p-type and n-type channel Cu-doped SnO provided by an embodiment of the present invention. The experimental results show that the logic circuit achieves an ultra-high voltage gain of 302.4 at a driving voltage of 50V.

[0117] Fig. 9 A performance diagram of a complementary logic circuit based on p-type and n-type channel Cu-doped SnO at a driving voltage of 50V provided in an embodiment of the present invention in terms of working stability and bending reliability test. The horizontal axis represents the bending radius, and the vertical axis represents the gain (left) and conversion voltage (right) at different bending radii. The experimental results show that even if placed in the air for one month, the device prepared by the present invention still maintains good working stability and bending reliability.

[0118] In summary, the present invention provides a method for preparing a complementary logic circuit based on p-type and n-type channel Cu-doped SnO, which successfully realizes the successful preparation of a logic circuit using a single metal oxide semiconductor.

[0119] Compared with the prior art, the technical solution conceived by the present invention can achieve the following beneficial effects:

[0120] 1. In hafnium oxide (HfO 2 ) After packaging, the Cu 3at% :Sn film was annealed to obtain n-type channel Cu 3at% :SnO thin film transistor. Due to the strong reducing property of Hf atoms, O atoms near the Sn vacancies migrate to the hafnium oxide layer, which suppresses the p-type conductivity in SnO. In addition, Cu 1+It can induce the formation of n-type doping effect and suppress electron-electron scattering by eliminating the degeneracy of conduction band energy level. 3at% The electron mobility of SnO thin film transistors reaches 43.8 cm 2 V -1 s -1 Above, the current switching ratio reaches 6.8×10 4 above.

[0121] 2. Directly on Cu 3at% :Sn thin film can be annealed to obtain p-type channel Cu 3at% :SnO thin film transistor, and then grow a hafnium oxide layer on the surface of the transistor. By plasma treating the device in an argon environment, Hf can be migrated to the Cu:SnO thin film, so that the threshold voltage of the device moves in the negative direction, and an enhanced p-type channel Cu is obtained. 3at% :SnO thin film transistor, its hole mobility reaches 2.4cm 2 V -1 s -1 Above, the current switching ratio reaches 1.3×10 4 above.

[0122] 3. In n-type and p-type channel Cu 3at% : On the basis of SnO thin film transistors, a complementary logic circuit based on p-type and n-type channel Cu-doped SnO was successfully prepared. The logic circuit prepared by the present invention has an ultra-high voltage gain of 302.4, as well as excellent working stability and bending reliability, and successfully realizes a complementary logic circuit based on a metal oxide semiconductor on a flexible substrate.

[0123] The above embodiments are only preferred embodiments of the present invention and cannot be used to limit the implementation mode and protection scope of the present invention. For those skilled in the art, after understanding the contents and principles of the specification of the present invention, any equivalent replacements and changes made thereto by them should be included in the protection scope of the present invention.

Claims

1. A method for preparing an n-type channel Cu-doped SnO thin film transistor, Features: The method comprises: Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer; Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer to obtain a Cu:Sn film; Step three, depositing an electrode layer on the surface of the Cu:Sn film; Step 4, growing a hafnium oxide layer on the surface of the device obtained in step 3; Step five: annealing to obtain an n-type channel Cu-doped SnO thin film transistor.

2. The method for preparing an n-type channel Cu-doped SnO thin film transistor according to claim 1, Features: The n-type channel Cu-doped SnO thin film transistor is obtained by annealing in air for a certain period of time after the hafnium oxide layer is deposited.

3. An n-type channel Cu-doped SnO thin film transistor, Features: The n-type channel Cu-doped SnO thin film transistor is prepared according to the method for preparing an n-type channel Cu-doped SnO thin film transistor according to claim 1.

4. A method for preparing a p-type channel Cu-doped SnO thin film transistor, Features: The method comprises: Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer; Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer to obtain a Cu:Sn film; Step 3: annealing to obtain a p-type Cu-doped SnO channel material; Step 4, depositing an electrode layer on the surface of the p-type Cu-doped SnO channel material to obtain a p-type channel Cu-doped SnO thin film transistor; Step 5, growing a hafnium oxide layer on the surface of the thin film transistor to obtain a p-type channel Cu-doped SnO thin film transistor; Step six, using a plasma cleaning machine to perform plasma treatment on the p-type channel Cu-doped SnO thin film transistor obtained in step five in an argon environment, so as to achieve regulation of the threshold voltage.

5. A p-type channel Cu-doped SnO thin film transistor, Features: The p-type channel Cu-doped SnO thin film transistor is prepared according to the method for preparing a p-type channel Cu-doped SnO thin film transistor according to claim 4.

6. A method for preparing SnO complementary logic circuit based on p-type and n-type channel Cu doping, Features: The method comprises: Step 1, sequentially manufacturing a substrate, a back gate electrode layer, and a gate dielectric layer; Step 2, depositing a Cu-doped metal Sn film on the surface of the gate dielectric layer, and obtaining a p-type Cu:SnO channel material after annealing; Step 3, depositing a Cu-doped metal Sn film next to the p-type Cu:SnO channel material; Step 4, depositing an electrode layer on the surface of the device after completing step 3 to obtain a p-type channel Cu:SnO thin film transistor; Step 5, growing a hafnium oxide layer on the surface of the device obtained in step 4; Step six, annealing to obtain n-type Cu-doped SnO channel material, and obtain a complementary logic circuit based on p-type and n-type channel Cu-doped SnO; Step seven: using a plasma cleaning machine to perform plasma treatment on the complementary logic circuit in an argon environment to achieve regulation of the threshold voltage.

7. The preparation method according to claim 6, Features: The p-type Cu:SnO channel material is obtained by annealing in air for a certain time before the hafnium oxide layer is deposited; the n-type Cu-doped SnO channel material is obtained by annealing in air for a certain time after the hafnium oxide layer is deposited.

8. A complementary logic circuit based on p-type and n-type channel Cu-doped SnO, Features: The complementary logic circuit is prepared according to the method for preparing a SnO complementary logic circuit based on p-type and n-type channel Cu doping according to claim 6.

9. The complementary logic circuit according to claim 8, Features: The substrate is a flexible substrate.