Thick steel plate for building structure and production method thereof
Through specific chemical composition and process flow, the thickness and mechanical properties of thick steel plates for building structures are improved, and the problem of insufficient thickness and strength in the existing technology is solved, and the steel plate with a thickness of 160mm is achieved to meet the requirements of high-level mechanical properties.
Patent Information
- Application Number
- CN202410204668.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-02-24
AI Technical Summary
The thickness and strength of the thick steel plates for existing building structures are difficult to meet the needs of super high-rise buildings and large-scale complex buildings, especially the mechanical performance requirements of the Q460GJ level, with a maximum thickness specification of only 150mm.
Using specific chemical composition combinations and process flows, including converter smelting, LF furnace refining, RH/VD vacuum treatment, continuous casting, rolling and heat treatment, control the chemical composition and structure of the steel plate, and add Nb, V, Ti, Al, etc. Microalloy elements improve the yield strength and tensile strength of the steel plate through gap solution strengthening and replacement solution strengthening, and stabilize the tissue performance through normalized and fast cooling and tempered heat treatment.
The steel plate with a thickness of 160mm is produced, meeting the mechanical properties requirements of the Q460GJ level, including yield strength 440~580MPa, tensile strength 550~720MPa, elongation ≥18%, yield strength ratio ≤0.83, 180° cold bending and impact performance , meets the quality level requirements of GB/T19879 and GB/T5313.
Smart Images

Figure CN117987733B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a thick steel plate for building structure and a production method thereof. Background Art
[0002] With the development of high-rise and super high-rise buildings, the demand for thick steel plates for building structures is becoming more and more urgent, especially for box columns in super high-rise buildings. In addition, large complex buildings also use a large number of special thick steel plates for building structures.
[0003] In recent years, the strength level and thickness requirements of thick steel plates for building structures have continued to increase. The maximum thickness specification of thick steel plates Q460GJ for building structures in GB / T19879-2015 is 150mm. Summary of the invention
[0004] The object of the present invention is to provide a thick steel plate for building structure and a production method thereof, wherein the thickness specification of the produced steel plate is 110-160 mm and meets the mechanical property requirements of Q460GJ.
[0005] The technical solution of the present invention:
[0006] A thick steel plate for building structure, the chemical composition of the steel is C=0.16%~0.18%, Si=0.20%~0.50%, Mn=1.50%~1.60%, P≤0.015%, S≤0.005%, Cr=0.20%~0.30%, Nb=0.040%~0.050%, V=0.055~0.065%, Ti=0.008%~0.020%, Al=0.020%~0.050%, B=0.0012~0.0020%, H≤0.0002%, N≤0.0090%, O≤0.0012%, the rest are Fe and unavoidable impurities, CEV≤0.54%; steel plate yield strength 440~580MPa, tensile strength 550~720MPa, elongation ≥18%, yield strength ratio ≤0.83, meets 3a radius 180° cold bending, 20, 0, -20℃ impact Akv≥47J, Z-direction surface shrinkage ≥35%.
[0007] Optimized, the chemical composition of the steel is C=0.17%~0.18%, Si=0.20%~0.30%, Mn=1.50%~1.55%, P≤0.012%, S≤0.003%, Cr=0.20%~0.25%, Nb=0.040%~0.045%, V=0.055~0.060%, Ti=0.012%~0.018%, Al=0.030%~0.050%, B=0.0012~0.0020%, H≤0.0002%, N≤0.0050%, O≤0.0012%, the rest are Fe and unavoidable impurities, CEV≤0.50%.
[0008] A method for producing thick steel plates for building structures, the key process steps comprising:
[0009] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1570-1620℃, converter tapping P≤0.008%, add deoxidizer and alloy for deoxidation and alloying during tapping, and use low P alloy to avoid P increase in molten steel.
[0010] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted. Then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit. H≤0.00015%, N≤0.0050%, O≤0.0010%.
[0011] (3) Continuous casting: The overheating temperature of the tundish is 8-25℃. Dynamic light pressure reduction or heavy pressure reduction technology is used to improve the internal quality of the continuous casting billet. The electric stirring at the end is used to control segregation. The thickness of the continuous casting billet is 350-450mm and the width is 1700-2500mm.
[0012] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1180 ~ 1250 ° C, furnace time ≥ 420 min.
[0013] (5) Rolling: Two-stage controlled rolling is adopted, the rough rolling temperature is 1200~1050℃, the rough rolling cumulative reduction ratio is ≥1.6, the intermediate billet thickness is 180~220mm, the finishing rolling start temperature is 850~890℃, the finishing rolling cumulative reduction ratio is ≥1.2, and the finishing rolling final rolling temperature is 790~820℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is ≥250℃, and the pile-cooling time is ≥48h.
[0014] (6) Heat treatment: normalizing fast cooling + tempering process, normalizing heating temperature 880 ~ 930 ℃, heating rate 1.6 ~ 2.2min / mm, holding time 20 ~ 50min, sectional roller quenching machine fast cooling; tempering heating temperature 500 ~ 600 ℃, heating rate 2.0 ~ 3.5min / mm, holding time 30 ~ 70min, tempering furnace stack cooling, stack cooling temperature ≥ 200 ℃, stack cooling time ≥ 16h.
[0015] Optimally, in step (3), the superheat of the tundish is 8-20°C, and the thickness of the continuous casting billet is 450 mm.
[0016] Optimally, in step (6), the normalizing heating temperature is 890-910°C, and the tempering heating temperature is 500-550°C.
[0017] Principle of the invention: The thick steel plate for building structures of the present invention has a thickness specification of 110 to 160 mm and is delivered in a heat-treated state. The chemical composition is based on C, Si, and Mn. Through interstitial solid solution strengthening and substitutional solid solution strengthening, the steel plate has the basic characteristics of low-alloy steel; adding appropriate amounts of micro-alloy elements such as Nb, V, Ti, and Al, on the one hand, refines the grains to achieve strength improvement, and on the other hand, improves strength through precipitation strengthening; through repeated experiments, it is confirmed that adding Cr and B to the steel plate to improve strength, on the one hand, improves the stability of supercooled austenite to refine the structure, and on the other hand, delays the transformation of ferrite and pearlite in the steel to increase the proportion of bainite structure; strictly control harmful elements such as P and S in the steel, and through LF, vacuum treatment, etc. Secondary refining improves the purity of steel, and electromagnetic stirring and dynamic reduction at the end of continuous casting improve the density of continuous casting billets; RH / VD vacuum treatment is used to reduce N in molten steel, and micro-alloying elements such as Al, Ti, and Nb are used to fix nitrogen to improve the role of effective B in steel; large-thickness cross-section continuous casting billets are used to ensure the compression ratio of the steel plate, improve the internal density of the steel plate and repair internal defects; normalizing and rapid cooling are used for steel plate heat treatment to ensure that the cooling rate at the in-thickness position of the steel plate can reach the cooling rate of air cooling of thin-gauge steel plates, thereby ensuring the structure and performance of the in-thickness position of the steel plate; tempering heat treatment of the steel plate further stabilizes the structure and performance.
[0018] Beneficial effects of the present invention: The thick steel plate for building structure of the present invention can have a maximum thickness of 160 mm, has good mechanical properties, and can meet the various performance indicators of quality grades C and D of Q460GJ in GB / T19879. The performance of the steel plate in the thickness direction meets the quality grade Z35 requirements in GB / T5313. The steel plate meets the mechanical performance requirements of Q460GJ, with a yield strength of 440-580 MPa, a tensile strength of 550-720 MPa, an elongation of ≥18%, a yield strength ratio of ≤0.83, and meets 3a radius 180° cold bending, 20°C, 0°C, -20°C impact Akv ≥47J, and Z-direction surface shrinkage ≥35%. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a metallographic structure photograph of the inner 1 / 4 thickness position of an embodiment of the present invention. The inner 1 / 4 and 1 / 2 thickness positions of the steel plate are ferrite and pearlite.
[0020] Figure 2 This is a metallographic structure photograph of the inner 1 / 2 thickness of Example 1 of the present invention. DETAILED DESCRIPTION
[0021] The following is an explanation with reference to embodiments.
[0022] The embodiment compares the process and performance of thick steel plates for building structures with four different chemical composition combinations, namely, Scheme ① to Scheme ④. The smelting chemical compositions are shown in Table 1.
[0023] Example 1
[0024] Using the chemical composition blank of Scheme ① in Table 1, the process steps are as follows:
[0025] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0026] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00012%, N≤0.0030%, and O≤0.0010%.
[0027] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0028] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 580 min.
[0029] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×3800mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 867℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 812℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 290℃, and the pile-cooling time is 62h.
[0030] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 930℃, the furnace time is 310min, and the steel is directly put into the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 500℃, the furnace time is 420min, and the tempering is stacked cooling after being taken out of the furnace. The stack cooling temperature is 220℃ and the stack cooling time is 26h.
[0031] Example 2
[0032] Using solution ① chemical composition blank, the process steps are as follows:
[0033] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0034] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00012%, N≤0.0030%, and O≤0.0010%.
[0035] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0036] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 620 min.
[0037] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 115×2900mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.8, the intermediate billet thickness is 160mm, the finishing rolling start temperature is 862℃, the finishing rolling cumulative reduction ratio is 1.39, and the finishing rolling final rolling temperature is 807℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 280℃, and the pile-cooling time is 50h.
[0038] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 930℃, the time in the furnace is 270min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 360min, and the tempering is stacked cooling after being taken out of the furnace, the stack cooling temperature is 220℃, and the stack cooling time is 24h.
[0039] Example 3
[0040] Using the chemical composition blank of Scheme ②, the process steps are as follows:
[0041] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1590℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0042] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted. Then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station. H≤0.00016%, N≤0.0035%, and O≤0.0010%.
[0043] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0044] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 670 min.
[0045] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×3660mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 880℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 800℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 300℃, and the pile-cooling time is 62h.
[0046] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 930℃, the time in the furnace is 300min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 500℃, the time in the furnace is 420min, and the tempering is stacked cooling after being taken out of the furnace. The stack cooling temperature is 230℃ and the stack cooling time is 28h.
[0047] Example 4
[0048] Using the chemical composition blank of Scheme ②, the process steps are as follows:
[0049] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1590℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0050] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted. Then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station. H≤0.00016%, N≤0.0035%, and O≤0.0010%.
[0051] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0052] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 650 min.
[0053] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×2780mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 873℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 280℃, and the pile-cooling time is 52h.
[0054] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 890℃, the time in the furnace is 300min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 420min, and the tempering is stacked cooling after being taken out of the furnace, the stacking cooling temperature is 230℃, and the stacking cooling time is 24h.
[0055] Example 5
[0056] Using the chemical composition blank of scheme ③, the process steps are as follows:
[0057] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0058] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted. Then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit. H≤0.00018%, N≤0.0040%, O≤0.0010%.
[0059] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0060] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 620 min.
[0061] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×2480mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 870℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 290℃, and the pile-cooling time is 52h.
[0062] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 890℃, the time in the furnace is 300min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 420min, and the tempering is stacked cooling after being taken out of the furnace, the stacking cooling temperature is 230℃, and the stacking cooling time is 24h.
[0063] Example 6
[0064] Using the chemical composition blank of scheme ③, the process steps are as follows:
[0065] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0066] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted. Then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit. H≤0.00018%, N≤0.0040%, O≤0.0010%.
[0067] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0068] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 710 min.
[0069] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×2970mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 873℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 280℃, and the pile-cooling time is 52h.
[0070] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 930℃, the time in the furnace is 310min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 420min, and the tempering is stacked cooling after being taken out of the furnace, the stacking cooling temperature is 230℃, and the stacking cooling time is 24h.
[0071] Example 7
[0072] Using the chemical composition blank of Scheme ④, the process steps are as follows:
[0073] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0074] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00010%, N≤0.0030%, and O≤0.0010%.
[0075] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0076] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 670 min.
[0077] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 140×2480mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.5, the intermediate billet thickness is 180mm, the finishing rolling start temperature is 873℃, the finishing rolling cumulative reduction ratio is 1.28, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 310℃, and the pile-cooling time is 52h.
[0078] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 890℃, the time in the furnace is 300min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 420min, and the tempering is stacked cooling after being taken out of the furnace, the stacking cooling temperature is 230℃, and the stacking cooling time is 24h.
[0079] Example 8
[0080] Using the chemical composition blank of Scheme ④, the process steps are as follows:
[0081] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0082] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00010%, N≤0.0030%, and O≤0.0010%.
[0083] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0084] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 650 min.
[0085] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 150×2480mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.25, the intermediate billet thickness is 200mm, the finishing rolling start temperature is 862℃, the finishing rolling cumulative reduction ratio is 1.33, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 320℃, and the pile-cooling time is 56h.
[0086] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 910℃, the time in the furnace is 350min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 430min, and the tempering is stacked cooling after being taken out of the furnace, the stack cooling temperature is 230℃, and the stack cooling time is 28h.
[0087] Example 9
[0088] Using the chemical composition blank of Scheme ④, the process steps are as follows:
[0089] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0090] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00010%, N≤0.0030%, and O≤0.0010%.
[0091] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0092] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 680 min.
[0093] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 160×2200mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.25, the intermediate billet thickness is 200mm, the finishing rolling start temperature is 863℃, the finishing rolling cumulative reduction ratio is 1.25, and the finishing rolling final rolling temperature is 805℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 320℃, and the pile-cooling time is 56h.
[0094] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 910℃, the time in the furnace is 360min, and it is directly cooled in a sectional roller quenching machine after being taken out of the furnace; the tempering heating temperature is 550℃, the time in the furnace is 430min, and the tempering is stacked cooling after being taken out of the furnace, the stack cooling temperature is 230℃, and the stack cooling time is 28h.
[0095] Example 10
[0096] Using the chemical composition blank of Scheme ④, the process steps are as follows:
[0097] (1) Converter smelting: top and bottom double blowing converter, control the tapping temperature at 1580℃, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during the tapping process, and the alloy uses low P alloy.
[0098] (2) Refining: After the molten steel in the ladle is heated by power supply in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas in the molten steel is measured at the exit station, and the H≤0.00010%, N≤0.0030%, and O≤0.0010%.
[0099] (3) Continuous casting: The overheating temperature of the tundish is 12-20°C. Dynamic light reduction or heavy reduction technology is used to improve the internal quality of the continuous casting billet. The final electric stirring is used to control segregation. The thickness of the continuous casting billet is 450 mm and the width is 2300 mm.
[0100] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1200 ~ 1250 ° C, furnace time 670 min.
[0101] (5) Rolling: Two-stage controlled rolling is adopted, and the finished product specification is 115×4560mm. The rough rolling temperature is 1166~1131℃, the rough rolling cumulative reduction ratio is 2.8, the intermediate billet thickness is 160mm, the finishing rolling start temperature is 887℃, the finishing rolling cumulative reduction ratio is 1.39, and the finishing rolling final rolling temperature is 812℃. The steel plate is pile-cooled after rolling, the pile-cooling temperature is 320℃, and the pile-cooling time is 56h.
[0102] (6) Heat treatment: The normalizing rapid cooling + tempering process is adopted. The normalizing heating temperature is 890℃, the time in the furnace is 280min, and it is directly sent to the segmented roller quenching machine for rapid cooling after being taken out of the furnace; the tempering heating temperature is 600℃, the time in the furnace is 360min, and the tempering is stacked cooling after being taken out of the furnace. The stack cooling temperature is 230℃ and the stack cooling time is 28h.
[0103] The performance test results of the steel produced in each embodiment are shown in Table 2 and Table 3.
[0104] Table 1 Example Scheme Smelting Chemical Composition (%)
[0105] .
[0106] Table 2 Test results of tensile properties and bending properties of the steel plates in the examples
[0107] .
[0108] Table 3 Impact performance and Z-direction performance test results of the steel plates of the examples
[0109] .
Claims
1. A method for producing thick steel plates for building structures, Features: The chemical composition of steel by weight percentage is C=0.17%~0.18%, Si=0.20%~0.30%, Mn=1.50%~1.55%, P≤0.012%, S≤0.003%, Cr=0.21%~0.25%, Nb=0.040%~0.045%, V=0.055~0.060%, Ti=0.012%~0.018%, Al=0.030%~0.050%, B=0.0012~0 .0020%, H≤0.0002%, N≤0.0050%, O≤0.0012%, the rest are Fe and unavoidable impurities, CEV≤0.50%; steel plate thickness 140~160mm, steel plate yield strength 440~505MPa, tensile strength 550~720MPa, elongation ≥18%, yield strength ratio ≤0.83, meet 3a radius 180° cold bending, 20, 0, -20℃ impact Akv≥47J, Z-direction surface shrinkage ≥35%; The process steps include: (1) Converter smelting: top and bottom double-blowing converter, control the tapping temperature at 1570-1620℃, converter tapping P≤0.008%, add deoxidizer and alloy for deoxidation and alloying during the tapping process; (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas H of the molten steel is measured at the exit station, which is ≤0.00015%, N ≤0.0050%, and O ≤0.0010%; (3) Continuous casting: The tundish superheat is 8-25°C, dynamic light reduction or heavy reduction technology is adopted, and the end-stage electric stirring is used to control segregation. The continuous casting billet thickness is 350-450mm and the width is 1700-2500mm; (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1250 ° C, soaking section temperature 1180 ~ 1250 ° C, furnace time ≥ 420 min; (5) Rolling: adopt two-stage controlled rolling, the rough rolling temperature is 1200~1050℃, the rough rolling cumulative compression ratio is ≥1.6, the intermediate billet thickness is 180~220mm, the finishing rolling start temperature is 850~890℃, the finishing rolling cumulative compression ratio is ≥1.2, and the finishing rolling final rolling temperature is 790~820℃; the steel plate is pile-cooled after rolling, the pile-cooling temperature is ≥250℃, and the pile-cooling time is ≥48h; (6) Heat treatment: normalizing fast cooling + tempering process, normalizing heating temperature 880 ~ 930 ℃, heating rate 1.6 ~ 2.2min / mm, holding time 20 ~ 50min, sectional roller quenching machine fast cooling; tempering heating temperature 500 ~ 600 ℃, heating rate 2.0 ~ 3.5min / mm, holding time 30 ~ 70min, tempering furnace stack cooling, stack cooling temperature ≥ 200 ℃, stack cooling time ≥ 16h.
2. The method for producing a thick steel plate for building structure according to claim 1, Features: In step (3), the superheat degree of the tundish is 8-20° C., and the thickness of the continuous casting billet is 450 mm.
3. The method for producing a thick steel plate for building structure according to claim 1, Features: In step (6), the normalizing heating temperature is 890-910°C, and the tempering heating temperature is 500-550°C.