Acidizing corrosion inhibitor and its preparation method and application

By introducing oxazole rings into the acidified corrosion inhibitor to form a stable adsorption film, the existing acidified corrosion inhibitors have been solved, and the problems of low efficiency and poor solvent recovery under high temperature conditions are achieved, and efficient metal surface corrosion protection is achieved. in the field of oil well acidification.

CN118005571BActive Publication Date: 2024-11-12SOUTHERN MARINE SCIENCE & ENGINEERING GUANGDONG LABORATORY (ZHANJIANG)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311792393.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-12
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The existing acidified corrosion inhibitors have low synthesis efficiency under high temperature conditions, poor solvent recovery rate, and insufficient corrosion protection effect on oil well carbon steel, which cannot meet the actual application needs.

Method used

An acidification corrosion inhibitor containing oxazole ring is used to form a uniform and stable adsorption film on the metal surface. The water solubility and adsorption are enhanced by heteroatoms N and O, thereby reducing the corrosion of corrosive substances on the metal surface. The synthesis conditions are mild and green.

Benefits of technology

In 20% HCl solution, the X65 steel sheet showed a corrosion inhibition rate of 98.65%. The synthesis route is simple, environmentally friendly, and has good applicability, making it easy to produce and apply on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118005571B_ABST
    Figure CN118005571B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of corrosion inhibitors, and particularly relates to an acidified corrosion inhibitor, a preparation method thereof and an application thereof. The structural formula of the acidified corrosion inhibitor of the present invention is: #imgabs0# wherein R1 and R2 independently represent any one of hydrogen, C1-C8 alkyl, C1-C8 alkyl derivative, phenyl and halogen. The acidified corrosion inhibitor of the present invention has a good corrosion inhibition effect on X65 steel sheet in 20% HCl solution. At 60°C, when the addition amount of the acidified corrosion inhibitor is 80ppm, the corrosion inhibition rate is as high as 98.65%. In addition, it affects the cathode and anode processes by adsorption on the electrode surface, and can form a uniform and stable adsorption film on the metal surface without changing the properties of the solution, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of corrosion inhibitors, and particularly relates to an acidifying corrosion inhibitor and a preparation method and application thereof. Background Art

[0002] Oil well acidizing is one of the important technologies to increase oil production. Its principle is to pump high-temperature acid into the wellbore to dissolve carbonates and other substances in the rock formation to expand the existing flow channels and open new flow channels to the wellbore to restore and maximize production. Oil wells are usually made of carbon steel. According to the nature of the well and the previous treatment, the most commonly used acids in acidizing treatment are hydrochloric acid (HCl), hydrofluoric acid (HF), acetic acid (CH3COOH), chloroacetic acid (ClCH2COOH), formic acid (HCOOH) and aminosulfonic acid (H2NSO3H), etc., but acidizing treatment will cause relatively serious corrosion to the carbon steel of the oil well. Therefore, adding corrosion inhibitors during acidizing treatment is the most practical, economical and effective anti-corrosion method. The presence of heteroatoms such as N, O, S, and P in organic compounds makes the corrosion inhibitor molecules form a film and adsorb on the metal surface, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances.

[0003] Common acidizing corrosion inhibitors include five-membered N-containing heterocyclics (imidazoline, pyrazole, oxazole, thiazole), quaternary ammonium salts, Schiff bases, Mannich bases, etc. However, the current acidizing corrosion inhibitors still cannot meet the demand for corrosion inhibition in practical applications, and the required temperature is high and the synthesis conditions are harsh. For example, imidazoline and its quaternary ammonium salt corrosion inhibitors have excellent properties such as low toxicity and high thermal stability and have been widely used in high-temperature acidizing operations, but the high temperature (up to 160°C), low efficiency, and poor solvent recovery rate faced in industrial synthesis have limited their further development.

[0004] Therefore, there is an urgent need to provide an acidified corrosion inhibitor which has good corrosion inhibition performance, mild synthesis conditions and is green. Summary of the invention

[0005] The present invention aims to solve one or more technical problems existing in the prior art, and at least provide a beneficial choice or create conditions. The present invention provides an acidified corrosion inhibitor, which has good corrosion inhibition performance, mild synthesis conditions and is green.

[0006] The inventive concept of the present invention is as follows: the acidified corrosion inhibitor of the present invention contains an oxazole ring, the heteroatoms N and O in the oxazole ring can enhance water solubility and adsorption, and the conjugated structure of the two benzene rings and the heteroatoms can form a uniform and stable adsorption film on the metal surface, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances, and having a good corrosion inhibition effect.

[0007] Therefore, a first aspect of the present invention provides an acidifying corrosion inhibitor.

[0008] Specifically, the structural formula of the acidifying corrosion inhibitor is:

[0009]

[0010] Here, R1 and R2 each independently represent any one of hydrogen, C1-C8 alkyl, C1-C8 alkyl derivative, phenyl, and halogen.

[0011] Preferably, the C1-C8 alkyl group includes any one of a methyl group and an ethyl group.

[0012] Preferably, the C1-C8 alkyl derivative includes any one of a methoxy group and an ethoxy group.

[0013] Preferably, the halogen includes any one of Cl and Br.

[0014] The second aspect of the present invention provides a method for preparing the acidifying corrosion inhibitor described in the first aspect of the present invention.

[0015] Specifically, the preparation method of the acidifying corrosion inhibitor comprises the following steps:

[0016] Reacting a1, a2 and an acid in a solvent to obtain the acidified corrosion inhibitor;

[0017] The structural formula of a1 is as follows:

[0018]

[0019] The structural formula of a2 is as follows:

[0020]

[0021] Preferably, the reaction temperature is 70-90°C, and the reaction time is 7-9h; further preferably, the reaction temperature is 75-85°C, and the reaction time is 7.5-8.5h; further preferably, the reaction temperature is 80°C, and the reaction time is 8h.

[0022] Preferably, the acid includes at least one of hydrochloric acid, Lewis acid, sulfuric acid, boric acid, and perchloric acid; more preferably, the acid is hydrochloric acid.

[0023] Preferably, the solvent includes at least one of dichloroethane, dimethyl sulfoxide and acetonitrile; more preferably, the solvent is acetonitrile.

[0024] Preferably, the mass ratio of a1 to a2 is 1:(1.4-2.2); further preferably, the mass ratio of a1 to a2 is 1:(1.6-2.0); further preferably, the mass ratio of a1 to a2 is 1:1.83.

[0025] Preferably, after the reaction is completed, the solvent is removed and the acidified corrosion inhibitor is obtained by column chromatography separation.

[0026] Preferably, the eluents used in the column chromatography separation are ethyl acetate and petroleum ether.

[0027] Preferably, the volume ratio of ethyl acetate to petroleum ether is 1:7.0-9.0; further preferably, the volume ratio of ethyl acetate to petroleum ether is 1:7.5-8.5; further preferably, the volume ratio of ethyl acetate to petroleum ether is 1:8.

[0028] Preferably, the preparation process of a1 is:

[0029] (1) mixing N-vinylformamide, an organic base, and a solvent, and stirring to obtain a mixture;

[0030] (2) adding a3 to the mixture obtained in step (1), reacting, then adding an inorganic base, continuing the reaction, extracting, and obtaining a1.

[0031] Preferably, in step (1), the molar ratio of N-vinylformamide to the organic base is 1:(1.0-1.4); further preferably, the molar ratio of N-vinylformamide to the organic base is 1:(1.1-1.3); further preferably, in step (1), the molar ratio of N-vinylformamide to the organic base is 1:1.2.

[0032] Preferably, the organic base comprises triethylamine.

[0033] Preferably, in step (1), the stirring is ice bath stirring.

[0034] Preferably, the solvent comprises tetrahydrofuran.

[0035] Preferably, in step (2), after a3 is added to the mixture, the reaction temperature is lower than 5°C, and the reaction time is 0.8-1.2 h; further preferably, the reaction temperature is 0-4.5°C, and the reaction time is 0.9-1.1 h.

[0036] Preferably, the molar ratio of N-vinylformamide to a3 is 1:1.3-1.7; further preferably, the molar ratio of N-vinylformamide to a3 is 1:1.4-1.6; further preferably, the molar ratio of N-vinylformamide to a3 is 1:1.5.

[0037] Preferably, in step (2), the inorganic base includes at least one of sodium hydroxide and potassium hydroxide; further preferably, the inorganic base is sodium hydroxide.

[0038] Preferably, the reaction time after adding the inorganic base in step (2) is 1.5-2.5 h; further preferably, the reaction time is 1.8-2.2 h; further preferably, the reaction time is 2 h.

[0039] Preferably, after the extraction is completed, the solvent is removed by a rotary evaporator, and then dried to obtain the a1.

[0040] Preferably, the structural formula of a3 is:

[0041]

[0042] Specifically, the organic base is added first, and then the inorganic base is added. The organic base triethylamine reacts relatively mildly in the acyl chloride, can remove the chlorine atom and avoid an overly violent reaction.

[0043] Preferably, the preparation process of a2 is:

[0044] (1) mixing potassium tert-butoxide, trimethyl sulfoxide iodide, and a solvent, and reacting to obtain a mixture;

[0045] (2) adding a4 to the mixture obtained in step (1), reacting, extracting, and obtaining a2.

[0046] Preferably, in step (1), the molar ratio of potassium tert-butoxide to trimethyl sulfoxide iodide is 4:2.5-3.5; further preferably, in step (1), the molar ratio of potassium tert-butoxide to trimethyl sulfoxide iodide is 4:2.7-3.3; further preferably, in step (1), the molar ratio of potassium tert-butoxide to trimethyl sulfoxide iodide is 4:3.

[0047] Preferably, in step (1), the solvent comprises tetrahydrofuran.

[0048] Preferably, in step (1), the reaction time is 1.5-2.5 h; further preferably, the reaction time is 1.8-2.2 h; further preferably, the reaction time is 2 h.

[0049] Preferably, in step (1), the reaction is carried out in an inert gas atmosphere.

[0050] Preferably, in step (2), the mixture is first cooled in an ice bath and then a4 is added.

[0051] Preferably, the molar ratio of a4 to trimethyl sulfoxide iodide is 1:0.8-1.2; further preferably, the molar ratio of a4 to trimethyl sulfoxide iodide is 1:0.9-1.1; further preferably, the molar ratio of a4 to trimethyl sulfoxide iodide is 1:1.

[0052] Preferably, in step (2), after a4 is added to the mixture, the system is first naturally heated to room temperature and then stirred.

[0053] Preferably, the stirring time is 2.5-3.5 h; further preferably, the stirring time is 2.7-3.3 h; further preferably, the stirring time is 3 h.

[0054] Specifically, the substances react during the stirring process.

[0055] Preferably, after the extraction is completed, the solvent is removed by a rotary evaporator and dried to obtain a2.

[0056] Preferably, the structural formula of a4 is:

[0057]

[0058] The third aspect of the present invention provides a use of the acidifying corrosion inhibitor described in the first aspect of the present invention in the field of corrosion protection.

[0059] Preferably, the anti-corrosion field includes the oil well acidizing field.

[0060] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0061] (1) The acidified corrosion inhibitor of the present invention contains an oxazole ring and is an oxazoline corrosion inhibitor. The heteroatoms N and O in the oxazole ring can enhance water solubility and adsorption. The conjugated structure of the two benzene rings and the heteroatoms can form a uniform and stable adsorption film on the metal surface, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by the corrosive substances, and having a good corrosion inhibition effect.

[0062] (2) The acidified corrosion inhibitor of the present invention has a good corrosion inhibition effect on X65 steel sheet in 20% HCl solution. At 60°C, when the addition amount of the acidified corrosion inhibitor is 80 ppm, the corrosion inhibition rate is as high as 98.65%. In addition, it affects the cathode and anode processes by adsorption on the electrode surface, and can form a uniform and stable adsorption film on the metal surface without changing the properties of the solution, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances.

[0063] (3) The present invention has a simple synthesis route, mild synthesis conditions, and the required solvents and additives are green and environmentally friendly, friendly to the human body and the environment. In addition, the preparation process is simple, the synthesis efficiency is high, the substrate applicability is good, and it is convenient for large-scale production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 The synthetic route of N-vinyl amide of Example 1 of the present invention is shown in FIG.

[0065] Figure 2 The synthetic route of the oxysulfur ylide of Example 1 of the present invention;

[0066] Figure 3 The synthetic route of the acidifying corrosion inhibitor of Example 1 of the present invention;

[0067] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of the acidified corrosion inhibitor of Example 1 of the present invention;

[0068] Figure 5 This is the carbon nuclear magnetic resonance spectrum of the acidified corrosion inhibitor of Example 1 of the present invention;

[0069] Figure 6 This is a corrosion inhibition performance curve diagram of the acidified corrosion inhibitor of Example 1 of the present invention;

[0070] Figure 7 This is the electrochemical polarization curve of X65 steel in 20% HCl with acidified corrosion inhibitor added;

[0071] Figure 8 This is the Nyquist diagram of X65 steel in 20% HCl with added acidifying corrosion inhibitor. DETAILED DESCRIPTION

[0072] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0073] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0074] Example 1

[0075] An acidizing corrosion inhibitor, the structural formula of which is:

[0076]

[0077] The preparation method of the acidifying corrosion inhibitor comprises the following steps:

[0078] (1) Synthesis of N-vinylamide: In a 50 mL three-necked round-bottom flask, reactants were added in a molar ratio of 1:1.2 between N-vinylformamide and triethylamine (Et3N), and then 25 mL of tetrahydrofuran (THF) was added to obtain a mixture. The mixture was stirred in an ice bath at 0°C in a nitrogen atmosphere. 2-methylbenzoyl chloride was charged into a constant pressure funnel at a molar ratio of 1:1.15 between N-vinylformamide and 2-methylbenzoyl chloride and was added dropwise to the mixture within 15 minutes. The system was then allowed to react at 4°C for 1 hour, and then 6 mL of 5 mol / L sodium hydroxide solution was added and the reaction was continued for 2 hours. After the reaction was completed, extraction was performed, the solvent was removed by a rotary evaporator, and the mixture was dried to obtain a crude product of N-vinylamide. The synthetic route is shown in the following figure. Figure 1 As shown;

[0079] (2) Synthesis of oxysulfur ylides: In a 250 mL round-bottom flask, potassium tert-butoxide (t-BuOK) and trimethyl sulfoxide iodide were added in a molar ratio of 4:3, followed by 60 mL of tetrahydrofuran, and reacted for 2 hours in an argon atmosphere to obtain a mixture; after the reaction, the mixture was cooled to 0°C in an ice bath, and naphthoyl chloride and trimethyl sulfoxide iodide were slowly added dropwise in a molar ratio of 1:1, and the system was naturally heated to room temperature and stirred for 3 hours. After the reaction, extraction was performed, and the solvent was removed by a rotary evaporator and dried to obtain a crude product of oxysulfur ylides. The synthetic route is shown in the following figure. Figure 2 As shown;

[0080] (3) Synthesis of acidifying corrosion inhibitor: 1.61 g N-vinylbenzamide, 2.94 g oxysulfur ylide, 10 mL acetonitrile (CH3CN), and 1 mL 1 mol / L hydrochloric acid were added to a 50 mL round-bottom flask in sequence, and refluxed at 80°C for 8 h. After the reaction, the solvent was removed by a rotary evaporator, and a mixed solvent of ethyl acetate and petroleum ether was used as an eluent to obtain an acidifying corrosion inhibitor by column chromatography. The synthetic route is shown in the following figure. Figure 3 shown.

[0081] The nuclear magnetic resonance hydrogen spectrum of the acidified corrosion inhibitor is as follows Figure 4 As shown, the characterization results of nuclear magnetic resonance hydrogen spectrum are:

[0082] 1H NMR (400MHz, CDCl3) δ8.52(s,1H),8.03(dd,J=8.6,1.7Hz,1H),7.91(m,J=9.5,7.6,5.0Hz,4H),7.65-7.53(m,2H),7.34(td,J=7.6,1.4Hz,1H),7.26 -7.19(m,2H),5.50(d,J=6.3Hz,1H),4.60(p,J=6.6Hz,1H),2.63(s,3H),1.58(d,J=6.7Hz,3H).

[0083] The carbon NMR spectrum of the acidified corrosion inhibitor is as follows: Figure 5 As shown, the characterization results of the carbon nuclear magnetic resonance spectrum are:

[0084] 13 C NMR (101MHz, CDCl3) δ195.38,163.18,139.07,135.89,132.42,131.77,131.27,130.86,130.83,130 .20,129.74,129.05,128.90,127.92,127.13,126.64,125.68,124.16,85.43,66.59,21.97,21.78.

[0085] Performance Testing

[0086] 1. Static coupon weight loss corrosion test

[0087] According to the normal pressure static corrosion rate measurement conditions and corrosion inhibitor evaluation indicators in the petroleum and natural gas industry standard SY / T 5405-2019 "Test Method and Evaluation Standard for Performance of Corrosion Inhibitors for Acidification", the corrosion inhibition performance of the acidification corrosion inhibitor obtained in Example 1 was tested by the static hanging plate weight loss method. The specific test method is as follows:

[0088] A standard X65 steel sheet was selected as the test object, with a specification of 50 mm × 10 mm × 3 mm. The steel sheet was first immersed in petroleum ether for 8 minutes to remove low-polarity grease, and then the steel sheet was taken out and immersed in anhydrous ethanol and acetone for 5 minutes respectively, dried with cold air and wrapped with filter paper, and then placed in a vacuum drying oven for 20 minutes, and weighed (the mass was accurate to 0.0001 g). The acidified corrosion inhibitor obtained in Example 1 with different concentrations was dissolved in a 20% mass fraction hydrochloric acid solution, and the mass fractions of the acidified corrosion inhibitor were determined to be 0.02wt% (20ppm) and 0.01wt% (20ppm). The corrosion rate and inhibition rate of X65 steel sheet at 0.04wt% (40ppm), 0.06wt% (60ppm), and 0.08wt% (80ppm) were measured. The experimental temperature was 60℃ and the measurement time was 4h. After the test, the steel sheet was taken out, and the impurities such as HCl on the surface of the steel sheet were dissolved with water. Then, the steel sheet was immersed in anhydrous ethanol and acetone for 5min respectively, and finally dried in a vacuum drying oven for 20min. The steel sheet was taken out and weighed (with the mass accurate to 0.0001g), and then the corrosion rate (r corr ) and corrosion inhibition rate (η).

[0089] The corrosion rate is calculated as follows:

[0090]

[0091] Among them, r corr is the corrosion rate of steel sheet / (g / m 2 / h); m is the weight of the steel sheet before the test / g; m t is the weight of the steel sheet after the test / g; mass loss ΔW = mm t ; 87600 is the calculation constant; S1 is the surface area of ​​the steel sheet / cm 2 ; T is the test time / h; ρ is the density of the steel sheet / (g / cm 3 ).

[0092] The calculation formula of corrosion inhibition rate is as follows:

[0093]

[0094] Wherein, η is the corrosion inhibition rate / %; Δm0 is the mass loss of the blank group steel sheet / g; Δm1 is the mass loss of the steel sheet after adding the acidified corrosion inhibitor / g.

[0095] The corrosion inhibition performance test results of the acidified corrosion inhibitor of Example 1 are shown in Table 1.

[0096] Example 1 The corrosion inhibition performance curve of the acidified corrosion inhibitor (corrosion rate and corrosion inhibition rate curve with the change of corrosion inhibitor concentration) is as follows Figure 6 shown.

[0097] Table 1: Corrosion inhibition performance test results of the acidified corrosion inhibitor prepared in Example 1

[0098]

[0099]

[0100] In Table 1, “-” indicates no corrosion inhibition rate.

[0101] From Table 1 and Figure 6 It can be seen that with the increase of acidification corrosion inhibitor concentration (from 0 to 0.08wt%), the mass loss of X65 steel sheet gradually decreases, and its corrosion rate increases from 476.5103g / m 2 / h reduced to 6.4138g / m 2 When the addition amount of the acidified corrosion inhibitor is 80 ppm (0.08 wt%), the corrosion inhibition rate of the X65 steel sheet is as high as 98.65%, indicating that the acidified corrosion inhibitor of the present invention can significantly slow down the corrosion rate of the steel sheet and has a good corrosion inhibition effect.

[0102] 2. Electrochemical corrosion test

[0103] The Donghua DH7000 electrochemical workstation was used with a three-electrode system. The acid-resistant mercurous sulfate electrode was used as the reference electrode and the platinum electrode was used as the auxiliary electrode. The circular end face with a diameter of 1 cm (working area 0.785 cm) was exposed in the epoxy resin sleeve. 2 ) X65 steel was used as the working electrode for testing. The AC impedance test frequency scanning range was 100000HZ~0.01HZ, and 10 frequencies were taken for each order of magnitude. The polarization curve test was performed by potential scanning from cathode to anode, the scanning range was ±0.2V relative to the open circuit potential, the scanning rate was 0.0005v / s, the AC amplitude was 0.01VRMS, and the computer automatically recorded the data; among them, there were 5 test groups, firstly, 20% mass fraction of hydrochloric acid was added to 5 200mL beakers, and then 0, 20, 40, 60, 80ppm of acidizing corrosion inhibitor were added to each beaker respectively.

[0104] The electrochemical corrosion performance test results of the acidified corrosion inhibitor obtained in Example 1 are shown in Table 2.

[0105] The electrochemical polarization curve of X65 steel in 20% HCl with acidified corrosion inhibitor is shown in Figure 7 As shown in the figure, Blank means no acidizing corrosion inhibitor is added, and the horizontal axis log i (A / cm 2 ) represents the corrosion current density, and the vertical axis E / V (vs. SCE) represents the corrosion potential.

[0106] Table 2: Electrochemical corrosion performance test results of the acidified corrosion inhibitor prepared in Example 1

[0107]

[0108]

[0109] Among them, b a represents the Tafel slope of the anodic curve, b c represents the cathode curve Tafel slope, i corr Indicates corrosion current, -E corr Indicates corrosion voltage, ΔE corr represents corrosion potential difference, IE represents corrosion inhibition efficiency, and “-” represents no data.

[0110] From Table 2 and Figure 7 It can be seen that after adding the acidified corrosion inhibitor, the current density of the cathode and the anode both decreases, indicating that the acidified corrosion inhibitor prepared in Example 1 of the present invention can simultaneously slow down the anodic dissolution process of the electrode reaction and the cathode hydrogen evolution reaction process. corr The oxazoline acidification corrosion inhibitor can effectively slow down the corrosion of metal by acid solution. Theoretically, when ΔE corr When ΔE is >85mV, the corrosion inhibition can be classified as an anodic corrosion inhibitor; corr When ΔE is less than -85mV, it can be classified as a cathodic corrosion inhibitor; corr When it is within the range of -85mV to +85mV, it is a mixed corrosion inhibitor. The ΔE of the acidified corrosion inhibitor prepared in Example 1 of the present invention is corr The value is within this range, indicating that the acidifying corrosion inhibitor of Example 1 of the present invention is a mixed corrosion inhibitor.

[0111] 3. AC impedance analysis

[0112] The AC impedance tester was used to test the AC impedance of X65 steel in 20% mass fraction HCl solution with different concentrations of acidified corrosion inhibitor. The Nyquist plot of X65 steel in 20% HCl with corrosion inhibitor is shown in Figure 2. Figure 8 As shown, the horizontal axis zˊ(Ω·cm 2 ) represents the real part of impedance, and the vertical coordinate zˊˊ(Ω·cm 2 ) represents the imaginary part of impedance, and Blank represents that no acidizing corrosion inhibitor is added.

[0113] Depend on Figure 8It can be seen that the AC impedance spectrum presents a semicircular single capacitance arc, indicating that the acidified corrosion inhibitor is an adsorption film type corrosion inhibitor. As the concentration of the oxazoline acidified corrosion inhibitor gradually increases, the impedance arc radius also increases, indicating that the oxazoline acidified corrosion inhibitor molecules cover the electrode surface more and more densely, and the shielding effect becomes stronger, thereby reducing the corrosion reaction rate. When the addition amount of the acidified corrosion inhibitor is 80ppm, the radius of the impedance semicircle is significantly greater than that of other concentrations, indicating that the acidified corrosion inhibitor has a significant corrosion inhibition effect at this concentration, and the entire electrochemical polarization curve is consistent with the static coupon weight loss corrosion test results.

[0114] In summary, the acidified corrosion inhibitor of the present invention has a good corrosion inhibition effect on X65 steel sheet in 20% HCl solution. At 60°C, when the corrosion inhibitor addition amount is 80ppm, the corrosion inhibition rate is as high as 98.65%. In addition, it affects the cathode and anode processes by adsorption on the electrode surface, and can form a uniform and stable adsorption film on the metal surface without changing the properties of the solution. It is a mixed corrosion inhibitor that inhibits both anode and cathode reactions, and can separate the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances. In addition, its synthesis route is simple, the synthesis conditions are mild, and the yield is high.

[0115] In addition, when the R1 substituent is any one of hydrogen, C2-C8 alkyl, C1-C8 alkyl derivative, phenyl, and halogen; when the R2 substituent is any one of hydrogen, C1-C8 alkyl, C1-C8 alkyl derivative, and halogen, the corrosion inhibition performance, electrochemical corrosion performance, and AC impedance test results of the corresponding acidifying corrosion inhibitor are similar to those of Example 1.

[0116] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An application of an acidifying corrosion inhibitor in the field of corrosion protection, characterized in that: The structural formula of the acidifying corrosion inhibitor is:

2. The use according to claim 1, characterized in that: The preparation method of the acidifying corrosion inhibitor comprises the following steps: Reacting a1, a2 and an acid in a solvent to obtain the acidified corrosion inhibitor; The structural formula of a1 is as follows: The structural formula of a2 is as follows:

3. The use according to claim 2, characterized in that: The reaction temperature is 70-90°C, and the reaction time is 7-9h.

4. The use according to claim 2, characterized in that: The acid is selected from at least one of hydrochloric acid, Lewis acid, sulfuric acid, boric acid and perchloric acid.

5. The use according to claim 2, characterized in that: The solvent is selected from at least one of dichloroethane, dimethyl sulfoxide and acetonitrile.

6. The use according to claim 2, characterized in that: The mass ratio of a1 and a2 is 1:(1.4-2.2).

7. The use according to any one of claims 2 to 6, characterized in that: After the reaction is completed, the solvent is removed and the acidified corrosion inhibitor is obtained by column chromatography separation.