A plasma-modified chitosan-cured epoxy soybean oil wood adhesive and its preparation method and application
Through the combination of plasma-modified chitosan and epoxy soybean oil, the problem of insufficient water resistance of formaldehyde release and bio-based adhesives in artificial boards was solved, and a fully biomass adhesive without any dext is developed to achieve efficient glue and water resistance. Reduce costs and conform to green chemistry trends.
Patent Information
- Application Number
- CN202410260521.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-03-07
AI Technical Summary
The formaldehyde resin adhesives widely used in the manufacturing of existing artificial boards have formaldehyde emission problems, which affects health and the environment. The water resistance of bio-based adhesives is insufficient, making it difficult to meet the application needs in humid environments.
Plasma modified chitosan is used to combine with epoxy soybean oil, and chitosan is treated by low-temperature plasma to promote the curing of epoxy soybean oil, form a completely biomass adhesive without any prescription, and improve the glue performance and water resistance.
It has achieved the development of a fully biomass adhesive without aldehydes, has excellent adhesive properties and water resistance, reduces the cost of adhesive, conforms to the trend of green chemistry and sustainable development, and is suitable for artificial boards and other wood bonding fields.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of artificial board production in wood processing, and in particular to a formula and application of a plasma-modified chitosan-cured epoxy soybean oil wood adhesive. Background Art
[0002] In the production process of modern man-made panels such as plywood, blockboard, particleboard, etc., adhesives play a vital role. Adhesives not only determine the production process and final application range of wood products, but also directly affect the production cost and the quality of the final product. They are the core of technological innovation in the man-made panel industry. The constant pursuit of adhesive performance, as well as the need to control costs and minimize environmental impact, constitute the main driving force for scientific and technological progress in this field.
[0003] At present, the artificial board manufacturing industry generally relies on resin adhesives synthesized based on formaldehyde, mainly including urea-formaldehyde (UF), phenol-formaldehyde (PF) and melamine-formaldehyde (MF) resins, as well as copolymers of these basic resins such as MUF, PUF, PMUF, etc. In particular, urea-formaldehyde resin has become the most widely used type of resin due to its excellent bonding performance and economic cost. However, the use of formaldehyde not only leads to the problem of formaldehyde emission in artificial board products, but also limits the application performance of the product due to the inherent instability of its chemical structure. According to studies, formaldehyde can cause irritation reactions to the eyes and upper respiratory tract after contact with the human body, and may lead to more serious health problems. The World Health Organization clearly pointed out in its Bulletin No. 153 issued in 2004 that formaldehyde is carcinogenic.
[0004] In order to reduce the formaldehyde emission in wood-based panel products, one of the most effective measures taken by the industry is to adjust the resin synthesis formula, especially to reduce the molar ratio of formaldehyde to urea (F / U). However, this improvement strategy is accompanied by a significant decrease in bonding performance, especially in terms of water resistance, which is far from meeting the application requirements in humid environments. Although resins such as PF, MF and MUF have also alleviated the formaldehyde emission problem to a certain extent, they have not been able to completely eradicate the problem of formaldehyde emission. The development of truly formaldehyde-free resins has become the ultimate goal of the industry. For example, although formaldehyde-free adhesives represented by isocyanate adhesives (such as pMDI) have been used to a certain extent in the production of wood-based panels, their application range is limited due to their high cost (tens of times higher than urea-formaldehyde resins) and high protection requirements during the production process. At present, the research focus has shifted to the preparation of green adhesives using renewable resources, such as adhesives based on soy protein and natural tannins. And through enzyme catalysis or chemical treatment of agricultural waste, lignin can be converted into phenolic compounds with good bonding properties, which can be used as basic components of adhesives. However, the above bio-based adhesives usually face the problem of insufficient water resistance, and the sustainable supply of raw materials is also a major challenge.
[0005] Chitosan, a natural high molecular weight polysaccharide extracted from crustaceans, has attracted extensive attention due to its good biocompatibility, biodegradability, non-toxicity and rich functional groups. These characteristics make the application of chitosan and its modified products in the field of adhesives one of the important directions of sustainable material research. Cross-linking modification is a common method to improve the bonding properties of chitosan. By reacting with multifunctional cross-linking agents such as glutaraldehyde, epichlorohydrin or isocyanate, a stable cross-linked network structure is formed between the chitosan molecular chains, thereby improving its bonding strength and water resistance as an adhesive. Graft copolymerization is another effective means to enhance the bonding properties of chitosan. By grafting polymer chains such as polyacrylic acid and polyvinyl alcohol on the main chain of chitosan, the bonding properties and flexibility of chitosan can be significantly improved. Esterification and etherification modifications mainly change the hydrophilicity and chemical stability of chitosan by introducing ester or ether groups, thereby improving its application performance under different environmental conditions. In addition, the bonding strength and environmental tolerance can be significantly improved by compounding with other natural polymers such as starch and cellulose.
[0006] In addition, inspired by epoxy resin adhesives, the use of epoxy ring-opening polymerization in epoxy oils to prepare adhesives has also attracted the attention of many scholars. The applicant has developed a co-cured epoxy soybean oil-based wood adhesive (CN202110377994.9) using epoxy soybean oil. Its bonding principle utilizes a large number of hydroxymethyl (-CH2-OH) in urea-formaldehyde resin polymers to undergo a ring-opening reaction with epoxy groups, and the hydroxyl groups generated by the ring-opening reaction can further react with epoxy groups of other oils and fats to polymerize. Therefore, the present invention utilizes an amino group (-NH2) exposed during the deacetylation process of each glucosamine unit in chitosan, and each glucosamine unit itself contains two hydroxyl groups (-OH). Both groups can act as nucleophiles to react with epoxy groups, and the epoxy bond reacts with the hydroxyl group to form a new ether bond (-COC-), the ring cracks and forms a new hydroxyl group, thereby accelerating the reaction. Chitosan reacts with amino groups to form a new amino ether bond (-C-NH-C-), and the ring-opening reaction between amino groups (-NH2) and epoxy groups (-O-) can occur in primary amines, secondary amines or tertiary amines and multifunctional amines. The various reactions of chitosan and epoxy oils lead to the formation of a three-dimensional network structure, which crosslinks and solidifies the resin to play a bonding role.
[0007] In order to promote the reaction between chitosan and epoxy oil, the present invention uses low-temperature plasma to attack the vulnerable parts of the polymer chain of chitosan, such as the glycosidic bonds between sugar rings or the carbon-carbon bonds on the long carbon chain, so that the long chain breaks and generates free radicals. The relatively small molecular weight glucose structure increases the reaction probability with the epoxy soybean oil, and promotes the curing process of the adhesive. In addition, the present invention uses plasma treatment to effectively increase the number of oxygen-containing groups such as hydroxyl and carboxyl groups on the surface of the treated material, and the introduction of highly active groups further promotes the curing of the epoxy soybean oil. The present invention solves a series of problems such as the difficulty in curing epoxy soybean oil and the poor adhesion of chitosan monomers. The broken chain chitosan as a curing agent for epoxy soybean oil promotes a polymer bonding network. The plasma-modified chitosan-cured epoxy soybean oil adhesive has excellent bonding properties, and the development of a formaldehyde-free all-biomass adhesive is realized.
[0008] Currently, there is a lack of a plasma-modified chitosan-cured epoxidized soybean oil wood adhesive and a preparation method and application thereof. Summary of the invention
[0009] The purpose of the present invention is to provide a wood adhesive of plasma-modified chitosan-cured epoxidized soybean oil and a preparation method and application thereof.
[0010] In order to solve the problems of the prior art, the present invention has the following technical solution: a plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention, the plasma-modified chitosan-cured epoxy soybean oil wood adhesive comprises component A and component B, and the plasma-modified chitosan-cured epoxy soybean oil wood adhesive comprises the following components in parts by weight:
[0011] Component A includes:
[0012] 70-76 parts of deionized water,
[0013] Chitosan powder 4-6 parts,
[0014] 20-24 parts of anhydrous acetic acid,
[0015] Component B is epoxidized soybean oil (ESO).
[0016] Furthermore, the deionized water meets the EW-IV grade and below standards of GB / T 11446.1-2013, the Mw of chitosan is 30000, DAC DEGREE≥85%, and the anhydrous acetic acid is analytically pure; and the epoxide value of the epoxidized soybean oil is ≥6.0.
[0017] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0018] (1) Weigh component A according to the stated weight proportions;
[0019] (2) dissolving chitosan powder and anhydrous acetic acid in deionized water, stirring for 3-5 hours at room temperature until the mixture is uniform, and obtaining a chitosan aqueous solution as component A;
[0020] (3) Component B is epoxidized soybean oil, and components A and B are kept aside to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0021] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0022] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60°C for 7-10 minutes, and repeat the above steps 1-4 times;
[0023] (2) The wood surface coated with component A is treated with sliding arc discharge plasma for 5-10 seconds;
[0024] (3) On the plasma treated A component coating, press 160-180g / m 2 Apply component B evenly and let it stand for 5 minutes;
[0025] (4) Place the surfaces to be bonded in a hot press at a temperature of 150-180°C and a pressure of 1 MPa for 5 minutes.
[0026] Furthermore, the plasma jet width is greater than the single board to be processed, and the plasma nozzle is 2-3 cm away from the single board.
[0027] Furthermore, the discharge power of the low-temperature plasma power supply is adjusted to 2000W, and glue can be applied to the activated surface within 30 minutes after treatment.
[0028] Furthermore, the plasma discharge method includes but is not limited to the sliding arc discharge method. The principle is that after treatment, the oxygen-containing groups such as hydroxyl groups on the surface of the wood board to be glued can be significantly increased and the long-chain structure of chitosan can be destroyed.
[0029] The invention discloses an application of the plasma modified chitosan solidified epoxy soybean oil wood adhesive in the preparation of artificial board.
[0030] Beneficial effects: The wood adhesive of the present invention has a simple preparation method, good bonding strength, and water resistance. All components of the adhesive are biomass materials, and it is a fully green and environmentally friendly adhesive. The cost is relatively low. The use method has no harsh conditions and is highly consistent with the production conditions of the existing wood-based panel production line, which can achieve effective integration with the existing technology and reduce the cost of the adhesive. All raw materials are biomass resources, and industrial mass production has been achieved.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] (1) The present invention first forms a layer of chitosan film on the wood bonding surface, and then solidifies the epoxy soybean oil by plasma modification of the chitosan film surface, thereby finally achieving the purpose of bonding wood. The bonding strength of the adhesive of the present invention is equivalent to that of mainstream chemical adhesives and has waterproof properties. The preparation of the adhesive makes full use of renewable resources - chitosan and soybean oil, among which chitosan is the second largest macromolecular substance in nature after cellulose, which not only reduces the dependence on traditional petrochemical resources, but also reduces the environmental impact during production and use. The concept of formaldehyde-free green adhesive is in line with the current trend of green chemistry and sustainable development.
[0033] (2) The invention of the adhesive provides a solution for curing epoxy grease. The epoxy soybean oil in the present invention is thoroughly cured and has good water resistance, which not only improves the immediate bonding strength, but also helps to improve the long-term stability and durability of the adhesive bonding interface. The invention provides a feasible development and application path for subsequent epoxy grease curing methods.
[0034] (3) The present invention introduces plasma treatment technology during the use of the adhesive. The introduction of this technology replaces the complex chemical reaction process and is a simple, green and environmentally friendly method. This innovative method effectively improves the bonding strength of the adhesive. The plasma modification method of the present invention is a sliding arc discharge plasma. The plasma use method is: activating the surface of the wood coated with component A for 5-10 seconds.
[0035] (4) The resin-pressed plywood prepared by the present invention can meet the requirements of the national standard GB / T 9846-2015 "Ordinary Plywood" for the water resistance of Class II boards, and can meet the requirements for the use of artificial board products in high humidity environments. At the same time, due to its good performance and environmental protection and ease of use, the adhesive is not only suitable for the artificial board industry, but is also expected to play an important role in furniture manufacturing and other fields requiring wood bonding. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme and advantages of this application clearer, the present invention is further described below in conjunction with embodiments, and the embodiments of the present invention include but are not limited to the following embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0037] Example 1
[0038] The invention discloses a plasma modified chitosan cured epoxy soybean oil wood adhesive. The plasma modified chitosan cured epoxy soybean oil wood adhesive comprises an A component and a B component. A poplar veneer with a thickness of 2 mm is used to make a three-layer plywood.
[0039] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0040] (1) Component A: Weigh the components according to weight ratio: 74 parts of deionized water, 6 parts of chitosan powder, and 20 parts of anhydrous acetic acid.
[0041] (2) Dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 3 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A.
[0042] (3) Component B is epoxidized soybean oil, and components A and B are on standby to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0043] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0044] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60℃ for 10 minutes and repeat the above steps once.
[0045] (2) The wood surface coated with component A was treated with sliding arc discharge plasma for 5 seconds.
[0046] (3) On the plasma treated A component coating, press 180g / m 2 Apply component B evenly and let it stand for 5 minutes.
[0047] (1) Place the surfaces to be bonded in a hot press at 160°C and 1 MPa for 5 minutes.
[0048] Example 2
[0049] The difference between Example 2 and Example 1 is that the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention is composed of component A and component B. Component A and component B are used separately to make a three-layer plywood using a poplar veneer with a thickness of 2 mm.
[0050] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0051] (1) Component A: Weigh the components according to weight ratio: 70 parts of deionized water, 6 parts of chitosan powder, and 24 parts of anhydrous acetic acid.
[0052] (2) Dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 4 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A.
[0053] (3) Component B is epoxidized soybean oil, and components A and B are on standby to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0054] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0055] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60℃ for 8 minutes and repeat the above steps once.
[0056] (2) The wood surface coated with component A was treated with sliding arc discharge plasma for 8 seconds.
[0057] (3) On the plasma treated A component coating, press 180g / m 2 Apply component B evenly and let it stand for 5 minutes.
[0058] (4) Place the surfaces to be bonded in a hot press at 160°C and 1 MPa for 5 minutes.
[0059] Example 3
[0060] The difference between Example 3 and Example 1 is that the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention is composed of component A and component B. Component A and component B are used separately to make a three-layer plywood using elm veneer with a thickness of 2 mm.
[0061] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0062] (1) Component A: Weigh the components according to weight ratio: 72 parts of deionized water, 6 parts of chitosan powder, and 22 parts of anhydrous acetic acid.
[0063] (2) Dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 3 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A.
[0064] (3) Component B is epoxidized soybean oil, and components A and B are on standby to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0065] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0066] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60℃ for 9 minutes and repeat the above steps once.
[0067] (2) The wood surface coated with component A was treated with sliding arc discharge plasma for 9 seconds.
[0068] (3) On the plasma treated A component coating, press 160g / m 2 Apply component B evenly and let it stand for 5 minutes.
[0069] (4) Place the surfaces to be bonded in a hot press at 180°C and 1 MPa for 5 minutes.
[0070] Example 4
[0071] The difference between Example 4 and Example 1 is that the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention is composed of component A and component B. Component A and component B are used separately to make a three-layer plywood using elm veneer with a thickness of 2 mm.
[0072] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0073] (1) Component A: Weigh the components according to the weight ratio, namely: 76 parts of deionized water, 4 parts of chitosan powder, and 20 parts of anhydrous acetic acid.
[0074] (2) Dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 3 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A.
[0075] (3) Component B is epoxidized soybean oil, and components A and B are on standby to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0076] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0077] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60℃ for 6 minutes and repeat the above steps 4 times.
[0078] (2) The wood surface coated with component A was treated with sliding arc discharge plasma for 5 seconds.
[0079] (3) On the plasma treated A component coating, press 180g / m 2 Apply component B evenly and let it stand for 5 minutes.
[0080] (4) Place the surfaces to be bonded in a hot press at 160°C and 1 MPa for 5 minutes.
[0081] Example 5
[0082] The plasma modified chitosan cured epoxy soybean oil wood adhesive of the invention consists of component A and component B. Component A and component B are used separately to make three-layer plywood with a pine veneer with a thickness of 2mm.
[0083] The preparation method of the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0084] (1) Component A: Weigh the components according to weight ratio: 73 parts of deionized water, 5 parts of chitosan powder, and 22 parts of anhydrous acetic acid.
[0085] (2) Dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 5 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A.
[0086] (3) Component B is epoxidized soybean oil, and components A and B are on standby to prepare plasma-modified chitosan-cured epoxidized soybean oil wood adhesive.
[0087] The method for using the plasma-modified chitosan-cured epoxy soybean oil wood adhesive of the present invention comprises the following steps:
[0088] (1) Apply 300g / m2 of pressure on the surface of the wood to be glued. 2 After evenly applying component A, dry it at 60℃ for 9 minutes and repeat the above steps twice.
[0089] (2) The wood surface coated with component A was treated with sliding arc discharge plasma for 10 seconds.
[0090] (3) On the plasma treated A component coating, press 170g / m 2 Apply component B evenly and let it stand for 5 minutes.
[0091] (4) Place the surfaces to be bonded in a hot press at a temperature of 150°C and a pressure of 1 MPa for 5 minutes.
[0092] Test Example 1
[0093] The plywood prepared in Examples 1-5 was taken respectively, and the physical and mechanical properties of the board were tested according to the national standard GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", and the standard used was the mechanical strength test standard for Class II plywood. The specific results are as follows: the wet bonding strength of the specimen after being soaked in 63°C hot water for 3 hours is 1.4-1.7Mpa, which meets and exceeds the national standard (≥0.7MPa).
[0094] According to the national standard GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", the 1m 3 The formaldehyde emission of the board was tested by the climate chamber method. The test results showed that the formaldehyde emission was 0mg / m 3 , no formaldehyde release.
[0095] Comparative Example 1
[0096] Patent "A water-based chitosan / citric acid supramolecular adhesive and its preparation method and application" (patent number: CN202310984517.8). This patent uses chitosan and citric acid as the main raw materials. The synthesis mechanism is that the amino group of chitosan and the carboxylate ions of citric acid are cross-linked to form a three-dimensional network structure, and after thermal curing, a bonding network is formed to act as an adhesive. The comparative patent is based on an acylation reaction, and a chitosan-citric acid complex is generated through an amide bond (-CONH-). The bonding principle of the present invention is the curing of epoxy soybean oil. In essence, chitosan provides the amino and hydroxyl groups required for the curing of epoxy oils, and the reaction mechanism is the ring-opening polymerization of epoxy bonds. At the same time, in order to improve the reactivity of chitosan, the long-chain chitosan is broken and modified by plasma. Therefore, the comparative patent and the present invention are completely different from the chemical reaction mechanism to the bonding process.
[0097] Comparative Example 2
[0098] Patent "A method for making formaldehyde-free bamboo board" (patent number: CN201810138976.3). This patent uses chitosan and konjac chitosan as the main raw materials, adds lysozyme to the A adhesive to adjust the molecular weight of chitosan, and then forms a complex with chitosan through fish gelatin for bonding; in adhesive B, soy protein and bone glue are also bonded, cross-linked or physically mixed to provide bonding force. The bonding principle is a complex reaction between chitosan and protein molecules to form a composite adhesive. Functional substances such as preservatives and montmorillonite are added to it. The product of this patent is a reconstituted bamboo board. The bonding principle of the adhesive of the present invention is the ring-opening polymerization of epoxy bonds as described in Comparative Example 1, and it is not targeted at specific wood products. Therefore, the comparative patent and the present invention are completely different from the chemical reaction mechanism to the bonding object.
[0099] Comparative Example 3
[0100] Patent "A co-cured epoxy soybean oil-based wood adhesive and its plasma enhancement method and application" (patent number: CN202110377994.9). This patent uses urea-formaldehyde resin to cure soybean oil, and the bonding principle is that the hydroxymethyl of the urea-formaldehyde resin is ring-opened and polymerized to the epoxy bond to form a thermosetting resin. The patent is consistent with the idea of the present invention in terms of bonding mechanism, but the ring-opening efficiency of urea-formaldehyde resin is far inferior to that of modified chitosan. At the same time, chitosan is not only used as a curing agent, but also forms a film distributed on the surface of the wood after being brushed on the surface of the wood and baked, which greatly improves the bonding relay of the present invention. Again, the adhesive of the comparative patent is an integrated solution, and the gluing process only needs to be brushed on the surface of the wood, while the adhesive of the present invention is divided into two substances, A and B. The two substances cannot be used alone, and must be brushed and hot-pressed in sequence according to the gluing scheme to achieve the gluing effect. The gluing process of the comparative patent and the present invention is completely different. Finally, both the comparative patent and the present invention use sliding arc plasma, but the plasma treatment object of the comparative patent is the wood surface, while the treatment object of the present invention is the chitosan film, the purpose of which is to break it into small molecular weight glucose units. From the above three comparisons, it can be concluded that the comparative patent and the present invention are completely different from each other in terms of chemical reaction mechanism and bonding object.
[0101] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and the scope of protection of the present invention is defined by the attached claims, description and their equivalents.
Claims
1. Application of plasma modified chitosan cured epoxy soybean oil wood adhesive in the preparation of artificial board, characterized in that The steps include: The plasma modified chitosan cured epoxy soybean oil wood adhesive comprises the following components in parts by weight: Component A includes: 70-76 parts of deionized water, Chitosan powder 4-6 parts, 20-24 parts of anhydrous acetic acid, Component B is epoxidized soybean oil ESO, (1) Weigh component A by weight; dissolve chitosan powder and anhydrous acetic acid in deionized water, and stir for 3-5 hours at room temperature until the mixture is uniformly mixed, to obtain a chitosan aqueous solution as component A; (2) Apply 300 g / m2 of pressure to the surface of the wood to be glued. 2 After applying component A evenly, dry it at 60℃ for 7-10 minutes, and repeat the above steps 1-4 times; The wood surface coated with component A was treated with gliding arc discharge plasma for 5-10 s. On the plasma treated A component coating, 160-180 g / m 2 Apply component B evenly and let it stand for 5 minutes; Place the surfaces to be bonded in a hot press at 150-180°C and 1MPa for 5 minutes.
2. The use according to claim 1, characterized in that: The plasma jet width is greater than the single board to be processed, and the plasma nozzle is 2-3 cm away from the single board.