Solid electrolyte membrane, preparation method and lithium ion battery
By introducing sulfides and high molecular weight PTFE binders into the solid electrolyte membrane and combining them with a polyolefin polymer precursor layer, the instability of PTFE binders to the negative electrode was solved, improving the mechanical and electrochemical performance of the battery and promoting the commercialization of solid-state batteries.
Patent Information
- Application Number
- CN202410417501.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-09
AI Technical Summary
In existing technologies, solid electrolyte membranes in lithium batteries suffer from the instability of PTFE binder on the negative electrode, leading to soft short circuits in the battery. Additionally, their thickness and lack of flexibility affect battery performance and energy density.
An electrolyte layer using sulfide and high molecular weight PTFE binder is combined with a polyolefin polymer precursor layer. By controlling the thickness and molecular weight of the polymer precursor layer, a three-dimensional network structure is formed, which enhances mechanical strength and ionic conductivity and avoids contact reaction between PTFE and the negative electrode.
This improves the mechanical properties, electrochemical stability, and interfacial stability of solid electrolyte membranes, enhances battery safety and cycle life, reduces material costs, and promotes the commercial application of solid-state batteries.
Smart Images

Figure CN118016982B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a solid electrolyte membrane, a preparation method and a lithium ion battery. Background Art
[0002] The electrolyte membrane is an indispensable part of lithium batteries, which separates the positive and negative electrodes and their active materials. The solid electrolyte membrane prepared by the dry method does not need to introduce solvents, which can reduce costs and avoid the adverse effects of solvents on electrolytes. Among them, inorganic solid electrolytes have high ionic conductivity, but because they are inorganic substances, when dry film formation is adopted, it is often necessary to add PTFE binders with good fiberization ability and low difficulty in composite film formation with inorganic materials. However, when the PTFE binder contacts the negative electrode, due to the low potential of the negative electrode and the provision of electrons, the PTFE is reduced and decomposed to form a conductive network, causing the battery to be soft short-circuited.
[0003] In the existing technology, the mainstream solutions include: 1. The electrolyte membrane is obtained by powder pressing, but it is thick and not flexible, which is not only difficult to scale up and manufacture, but also the energy density of the obtained battery material is poor; 2. A small amount of PTFE is added to reduce side reactions, and non-woven fabric is added on one side to ensure mechanical properties. However, non-woven fabric is a poor conductor of ions and will affect the performance of the battery. Summary of the invention
[0004] The present invention provides a solid electrolyte membrane, a preparation method and a lithium ion battery, which not only maintain high ion conductivity but also solve the problem that a PTFE binder in the solid electrolyte membrane is unstable to a negative electrode.
[0005] To this end, a first object of the present invention is to provide a solid electrolyte membrane.
[0006] A second object of the present invention is to provide a method for preparing a solid electrolyte membrane.
[0007] A third object of the present invention is to provide a lithium ion battery.
[0008] To achieve the first objective of the present invention, the technical solution of the present invention provides a solid electrolyte membrane, comprising: an electrolyte layer, the electrolyte layer comprising: a sulfide and a PTFE binder; a polymer precursor layer, the polymer precursor layer is arranged on the side close to the negative electrode active material, the polymer precursor layer is formed after the polymer precursor is solidified, and the polymer precursor comprises: a polyene polymer.
[0009] Furthermore, the molecular weight of the PTFE binder is greater than 10000000. A PTFE binder with a large molecular weight can improve mechanical strength while ensuring the dosage.
[0010] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the electrolyte layer of the solid electrolyte membrane of the present invention includes sulfide, which has higher ionic conductivity, good mechanical properties, electrochemical stability and interface stability, and can cooperate with the polymer precursor layer to make the solid electrolyte membrane stronger. The polyene-based polymer in the polymer precursor layer forms a three-dimensional network structure after film formation, so that it can provide better mechanical support, enhance the structural stability of the solid electrolyte membrane, effectively resist external stress, and prevent the electrolyte membrane from breaking or being damaged during the battery cycle. It has higher strength and does not require the addition of poor conductors such as non-woven fabrics; its three-dimensional network structure helps the transmission of lithium ions, thereby improving the ionic conductivity of the electrolyte membrane; the polyene-based polymer can form a stable interface with lithium metal to reduce adverse reactions, thereby improving the safety and cycle life of the battery.
[0011] In one technical solution of the present invention, the thickness of the polymer precursor layer is 1 μm-5 μm.
[0012] Compared with the prior art, the technical effect achieved by adopting the technical solution is as follows: the present invention controls the tensile properties and electrochemical properties of the solid electrolyte membrane by controlling the thickness of the polymer precursor layer. When the thickness of the polymer precursor layer is greater than 5 μm, the tensile strength is high, but because the ionic conductivity of the polymer precursor layer is not as high as that of the sulfide solid electrolyte, the film formation is too thick, which will lead to the deterioration of the performance; when the thickness of the polymer precursor layer is less than 1 μm, the film formation is too thin, resulting in the inability to effectively avoid the contact reaction between the PTFE in the sulfide solid electrolyte and the negative electrode, resulting in the deterioration of the electrical performance; the present invention has found through a large number of studies that when the thickness of the polymer precursor layer is 1 μm-5 μm, the polymer precursor layer of appropriate thickness can maintain the stability of the solid electrolyte membrane while ensuring its good processability and interface contact, and at this time, the tensile properties, stability, interface compatibility between the electrolyte layer and the polymer precursor layer, interface compatibility between electrodes, and electrochemical performance of the solid electrolyte membrane are all improved overall.
[0013] In one technical solution of the present invention, the molecular weight of the polyene polymer is 600-1500.
[0014] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the present invention controls the tensile properties and electrochemical properties of the solid electrolyte membrane by controlling the molecular weight of the polyene-based polymer. For polyene-based polymers of the same mass, the molecular weight determines its fluidity, the number of monomers and the pores of its film formation, etc. The smaller the molecular weight, the more monomers there are, the more three-dimensional networks are formed during film formation, and the stronger the tensile properties are. However, too many three-dimensional networks will also make the solid electrolyte membrane harder, which is not conducive to interfacial contact and thus affects the electrochemical properties. For polyene-based polymers with a molecular weight of 600-1500, the fluidity and processability of the polymer are balanced, and the solid electrolyte membrane formed during the preparation process is uniform and defect-free; it helps to control the pore size and distribution of the polymer precursor layer, and the three-dimensional network and its tensile properties are moderate during film formation, thereby enhancing the electrochemical properties of the solid electrolyte membrane.
[0015] In a technical solution of the present invention, the polymer precursor includes, by weight: ionic liquid, 50-60 parts by weight; polyene polymer, 10-20 parts by weight; lithium salt, 20-30 parts by weight; initiator, 2-4 parts by weight.
[0016] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: in the polymer precursor of the present invention, the ratio of ionic liquid to lithium salt determines the ion conductivity of the electrolyte membrane. Under this ratio, it is helpful to form a better ion conduction channel, thereby improving the ion conductivity of the solid electrolyte; the addition of a small amount of polyene polymer can enhance the structural stability of the solid electrolyte membrane, reduce adverse reactions and increase mechanical strength; the addition of a trace amount of initiator helps to control the speed and degree of the polymerization reaction, thereby making the preparation process of the electrolyte membrane more controllable, which is conducive to the formation of a uniform and defect-free polymer precursor layer.
[0017] To achieve the second purpose of the present invention, the technical solution of the present invention provides a method for preparing a solid electrolyte membrane, and the preparation method includes the following steps: S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder evenly, and rolling them into a film to obtain an electrolyte layer; S200, in an inert gas protective atmosphere, preparing a polymer precursor; S300, coating the polymer precursor on the electrolyte layer, heating and curing it, to obtain a solid electrolyte membrane.
[0018] Further, the preparation method also includes: S400, under an inert gas protective atmosphere, weighing the ternary positive electrode material, sulfide solid electrolyte, PTFE binder and conductive carbon in a mass ratio of 60-90:10-40:0.1-10:1-5, grinding and mixing them evenly, and then repeatedly rolling them at 50-150°C with a roller press to obtain a positive electrode; S500, under an inert gas protective atmosphere, weighing the graphite negative electrode material, sulfide solid electrolyte, and PTFE binder in a mass ratio of 50-70:50-30:0.1-10, grinding and mixing them evenly, and then repeatedly rolling them at 50-150°C with a roller press to obtain a negative electrode; S600, placing the negative electrode, solid electrolyte membrane and positive electrode in an assembly device in turn, pressurizing, and obtaining a lithium-ion battery. It is worth noting that when performing the S600 assembly step, the polymer precursor layer of the solid electrolyte membrane is arranged close to the negative electrode side.
[0019] Furthermore, the preparation methods are all carried out in a glove box.
[0020] Compared with the prior art, the technical effect achieved by adopting the technical solution is as follows: It can be understood that in order to avoid its reaction with oxygen or water vapor in the air, the preparation method is carried out under an inert gas protective atmosphere. The sulfide solid electrolyte obtained by the preparation method of the present invention has high ionic conductivity and solves the problem that the PTFE binder in the solid electrolyte membrane is unstable to the negative electrode.
[0021] In a technical solution of the present invention, in S100, the added amount of PTFE binder is 0.1%-10% of the sulfide solid electrolyte; and / or in S100, the rolling temperature is 50°C-150°C.
[0022] Compared with the prior art, the technical effects achieved by adopting the technical scheme are as follows: the present invention controls the addition amount of the PTFE binder to ensure the structural stability and electronic conductivity of the material; the material is compacted by rolling to form a uniform and dense film layer, and the rolling temperature usually needs to be determined according to the characteristics of the electrolyte material. The present invention controls the rolling temperature between 50°C and 150°C, which has a positive impact on improving processing efficiency, enhancing mechanical properties, and optimizing electrochemical properties.
[0023] In a technical solution of the present invention, S200 specifically includes: under an inert gas protective atmosphere, adding ionic liquid, polyene polymer, lithium salt and initiator in order according to parts by mass, and stirring them uniformly to obtain a polymer precursor.
[0024] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the present invention can reduce the cost of material use while ensuring the overall performance through reasonable material ratios and reaction conditions, which is of great significance to the commercialization process of batteries.
[0025] In one technical solution of the present invention, the ionic liquid includes: at least one of 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, LiAsF6, LiPF6, LiBF6, and LiClO4; the polyene polymer includes: at least one of PEGDA, tripropylene glycol diacrylate, and tri(ethylene glycol) diacrylate; the lithium salt includes: at least one of LiTFSi, lithium bis(oxalatoborate), and lithium difluorooxalatoborate; the initiator includes: at least one of AIBN, dimethyl azobisisobutyrate, and benzoyl peroxide.
[0026] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: the ionic liquid of the present invention can provide freely moving ions, has high ionic conductivity and good thermal stability, thereby enhancing the ionic conductivity of the electrolyte membrane; the polyene-based polymer provides a skeleton structure in the solid electrolyte membrane, which helps to maintain the mechanical stability and flexibility of the membrane. These polymers can also form a three-dimensional network structure through a cross-linking reaction, further improving the stability and electrochemical properties of the electrolyte membrane; lithium salt plays the role of providing a lithium ion source in the solid electrolyte membrane, and is a key substance for realizing lithium ion transmission; the use of an initiator is crucial to controlling the speed and degree of the polymerization reaction, and is used to initiate the polymerization reaction, promote the cross-linking and curing of the polyene-based polymer, and form a stable solid electrolyte membrane. Through the various material components of the polymer precursor of the present invention, a solid electrolyte membrane with high ionic conductivity, good mechanical properties and excellent electrochemical stability can be prepared.
[0027] In a technical solution of the present invention, in S300, the temperature of heating and curing is 50°C-80°C; and / or in S300, the time of heating and curing is 12h-48h.
[0028] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: the present invention cross-links the polymer molecular chains through heat treatment to form a stable three-dimensional network structure, thereby improving the mechanical strength and chemical stability of the membrane. The temperature of heating and curing is based on the material properties and the requirements of the curing process. In this temperature range, it can be ensured that the polymer precursor can complete the cross-linking reaction under appropriate heat, while avoiding material degradation or other adverse reactions due to excessively high temperature; the setting of the heating and curing time is to ensure that the polymer precursor can fully complete the cross-linking reaction and achieve uniform curing. Too short a time may lead to incomplete curing and affect the performance of the electrolyte membrane; too long a time may increase energy consumption and production costs, and the marginal effect on improving material performance decreases.
[0029] To achieve the third objective of the present invention, the technical solution of the present invention provides a lithium-ion battery, comprising: a positive electrode active material, a negative electrode active material and a solid electrolyte membrane as described in any of the above technical solutions.
[0030] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the lithium-ion battery of this technical solution includes the solid electrolyte membrane of any technical solution of the present invention, and thus has all the beneficial effects of the solid electrolyte membrane of any technical solution of the present invention, which will not be repeated here.
[0031] The technical solution provided by the present invention can achieve at least one of the following effects:
[0032] (1) The solid electrolyte membrane of the present invention combines the advantages of inorganic solid electrolyte and polymer solid electrolyte, ensuring the high conductivity of its battery material;
[0033] (2) The polymer precursor layer in the solid electrolyte membrane of the present invention can not only provide better mechanical support, but also form a stable interface with the negative electrode active material, reduce adverse reactions, thereby improving the safety and cycle life of the battery, and help promote the commercialization of solid-state battery technology, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A SEM image of an uncured solid electrolyte membrane provided by an embodiment of the present invention;
[0035] Figure 2 This is a SEM image of the solid electrolyte membrane provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0036] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be noted that, in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other. In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and therefore, the protection scope of the present invention is not limited by the specific embodiments disclosed below.
[0037] Refer to the following Figure 1 to Figure 2 The technical solutions of some embodiments of the present invention are described.
[0038] An embodiment of the present invention provides a solid electrolyte membrane, comprising: an electrolyte layer, the electrolyte layer comprising: a sulfide and a PTFE binder; a polymer precursor layer, the polymer precursor layer is arranged near the negative electrode active material side, the polymer precursor layer is formed after the polymer precursor is solidified, and the polymer precursor comprises: a polyene polymer.
[0039] For example, the molecular weight of the PTFE binder is > 10000000. A high molecular weight PTFE binder can improve the mechanical strength while ensuring the dosage.
[0040] The electrolyte layer of the solid electrolyte membrane of the present invention includes sulfide, which has higher ionic conductivity, good mechanical properties, electrochemical stability and interface stability, and can cooperate with the polymer precursor layer to make the solid electrolyte membrane stronger. The polyene-based polymer in the polymer precursor layer forms a three-dimensional network structure after film formation, so that it can provide better mechanical support, enhance the structural stability of the solid electrolyte membrane, effectively resist external stress, and prevent the electrolyte membrane from breaking or being damaged during the battery cycle. The strength is higher and no poor conductors such as non-woven fabrics are added; its three-dimensional network structure helps the transmission of lithium ions, thereby improving the ionic conductivity of the electrolyte membrane; the polyene-based polymer can form a stable interface with lithium metal to reduce adverse reactions, thereby improving the safety and cycle life of the battery.
[0041] In some implementations of the examples of the present application, specifically, the thickness of the polymer precursor layer is 1 μm-5 μm.
[0042] The present invention controls the tensile properties and electrochemical properties of the solid electrolyte membrane by controlling the thickness of the polymer precursor layer. When the thickness of the polymer precursor layer is greater than 5 μm, the tensile strength is high, but because the ionic conductivity of the polymer precursor layer is not as high as that of the sulfide solid electrolyte, the film formation is too thick, which will lead to the deterioration of the performance; when the thickness of the polymer precursor layer is less than 1 μm, the film formation is too thin, resulting in the inability to effectively avoid the contact reaction between the PTFE in the sulfide solid electrolyte and the negative electrode, resulting in the deterioration of the electrical properties; the present invention has found through a large number of studies that when the thickness of the polymer precursor layer is 1 μm-5 μm, the polymer precursor layer of appropriate thickness can maintain the stability of the solid electrolyte membrane while ensuring its good processability and interface contact, and at this time, the tensile properties, stability, interface compatibility between the electrolyte layer and the polymer precursor layer, interface compatibility between electrodes, and electrochemical properties of the solid electrolyte membrane are all improved as a whole.
[0043] In some implementations of the examples of the present application, specifically, the molecular weight of the polyene polymer is 600-1500.
[0044] The present invention controls the tensile properties and electrochemical properties of the solid electrolyte membrane by controlling the molecular weight of the polyene polymer. For polyene polymers of the same mass, the molecular weight determines its fluidity, the number of monomers and the pores of its film formation, etc. The smaller the molecular weight, the more monomers there are, the more three-dimensional networks are formed during film formation, and the stronger the tensile properties are. However, too many three-dimensional networks will also make the solid electrolyte membrane harder, which is not conducive to interfacial contact and thus affects the electrochemical properties. For polyene polymers with a molecular weight of 600-1500, the fluidity and processability of the polymer are balanced, and the solid electrolyte membrane formed during the preparation process is uniform and defect-free; it helps to control the pore size and distribution of the polymer precursor layer, and the three-dimensional network and its tensile properties are moderate during film formation, thereby enhancing the electrochemical properties of the solid electrolyte membrane.
[0045] In some implementations of the examples of the present application, specifically, the polymer precursor includes, in parts by mass: ionic liquid, 50 parts by mass to 60 parts by mass; polyene polymer, 10 parts by mass to 20 parts by mass; lithium salt, 20 parts by mass to 30 parts by mass; initiator, 2 parts by mass to 4 parts by mass.
[0046] In the polymer precursor of the present invention, the ratio of ionic liquid to lithium salt determines the ion conduction capacity of the electrolyte membrane. At this ratio, it is helpful to form a better ion conduction channel, thereby improving the ion conductivity of the solid electrolyte; the addition of a small amount of polyene polymer can enhance the structural stability of the solid electrolyte membrane, reduce adverse reactions and increase mechanical strength; the addition of a trace amount of initiator helps to control the speed and degree of the polymerization reaction, thereby making the preparation process of the electrolyte membrane more controllable, which is conducive to the formation of a uniform and defect-free polymer precursor layer.
[0047] To achieve the second purpose of the present invention, an embodiment of the present invention provides a method for preparing a solid electrolyte membrane, the preparation method comprising the following steps: S100, under an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder evenly, and rolling them into a film to obtain an electrolyte layer; S200, under an inert gas protective atmosphere, preparing a polymer precursor; S300, coating the polymer precursor on the electrolyte layer, heating and curing it, to obtain a solid electrolyte membrane.
[0048] For example, the preparation method also includes: S400, under an inert gas protective atmosphere, weighing the ternary positive electrode material, sulfide solid electrolyte, PTFE binder and conductive carbon in a mass ratio of 60-90:10-40:0.1-10:1-5, grinding and mixing them evenly, and then repeatedly rolling them at 50-150°C with a roller press to obtain a positive electrode; S500, under an inert gas protective atmosphere, weighing the graphite negative electrode material, sulfide solid electrolyte, and PTFE binder in a mass ratio of 50-70:50-30:0.1-10, grinding and mixing them evenly, and then repeatedly rolling them at 50-150°C with a roller press to obtain a negative electrode; S600, placing the negative electrode, solid electrolyte membrane and positive electrode in an assembly device in turn, pressurizing, and obtaining a lithium-ion battery. It is worth noting that when performing the S600 assembly step, the polymer precursor layer of the solid electrolyte membrane is arranged close to the negative electrode side.
[0049] For example, the preparation methods are all carried out in a glove box.
[0050] It is understandable that in order to avoid reaction with oxygen or water vapor in the air, the preparation method is carried out under an inert gas protective atmosphere. The sulfide solid electrolyte obtained by the preparation method of the present invention has high ionic conductivity and solves the problem of instability of the PTFE binder to the negative electrode in the solid electrolyte membrane. Since the polymer precursor is relatively soft and the cured polymer precursor layer itself is also a good ion conductor, it is more conducive to the performance of the battery.
[0051] In some implementations of the examples of the present application, specifically, in S100, the amount of PTFE binder added is 0.1%-10% of the sulfide solid electrolyte; and / or in S100, the rolling temperature is 50°C-150°C.
[0052] The present invention controls the added amount of PTFE binder to ensure the structural stability and electronic conductivity of the material; the material is compacted by rolling to form a uniform and dense film layer, and the rolling temperature usually needs to be determined according to the characteristics of the electrolyte material. The present invention controls the rolling temperature between 50°C and 150°C, which has a positive effect on improving processing efficiency, enhancing mechanical properties, optimizing electrochemical properties, etc.
[0053] In some implementations of the examples of the present application, specifically, S200 specifically includes: under an inert gas protective atmosphere, adding the ionic liquid, the polyene polymer, the lithium salt and the initiator in order according to parts by mass, and stirring them evenly to obtain a polymer precursor.
[0054] The present invention can reduce the cost of material use while ensuring overall performance through reasonable material ratios and reaction conditions, which is of great significance to the commercialization process of batteries.
[0055] In some embodiments of the examples of the present application, specifically, the ionic liquid includes: at least one of 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, LiAsF6, LiPF6, LiBF6, and LiClO4; the polyene polymer includes: at least one of PEGDA, tripropylene glycol diacrylate, and tri(ethylene glycol) diacrylate; the lithium salt includes: at least one of LiTFSi, lithium bis(oxalatoborate), and lithium difluorooxalatoborate; the initiator includes: at least one of AIBN, dimethyl azobisisobutyrate, and benzoyl peroxide.
[0056] The ionic liquid of the present invention can provide freely moving ions, has high ionic conductivity and good thermal stability, thereby enhancing the ionic conductivity of the electrolyte membrane; the polyene-based polymer provides a skeleton structure in the solid electrolyte membrane, which helps to maintain the mechanical stability and flexibility of the membrane. These polymers can also form a three-dimensional network structure through a cross-linking reaction, further improving the stability and electrochemical performance of the electrolyte membrane; lithium salt plays the role of providing a lithium ion source in the solid electrolyte membrane, and is a key substance for realizing lithium ion transmission; the use of an initiator is crucial for controlling the speed and degree of the polymerization reaction, and is used to initiate the polymerization reaction, promote the cross-linking and curing of the polyene-based polymer, and form a stable solid electrolyte membrane. Through the various material components of the polymer precursor of the present invention, a solid electrolyte membrane with high ionic conductivity, good mechanical properties and excellent electrochemical stability can be prepared.
[0057] In some implementations of the examples of the present application, specifically, in S300, the temperature of heating and curing is 50°C-80°C; and / or in S300, the time of heating and curing is 12h-48h.
[0058] The present invention cross-links the polymer molecular chains through heat treatment to form a stable three-dimensional network structure, thereby improving the mechanical strength and chemical stability of the membrane. The temperature of heating and curing is based on the material properties and the requirements of the curing process. In this temperature range, it can be ensured that the polymer precursor can complete the cross-linking reaction under appropriate heat, while avoiding material degradation or other adverse reactions due to excessively high temperature. The setting of the heating and curing time is to ensure that the polymer precursor can fully complete the cross-linking reaction and achieve uniform curing. If the time is too short, it may lead to incomplete curing and affect the performance of the electrolyte membrane. If the time is too long, it may increase energy consumption and production costs, and the marginal effect on improving material performance will decrease.
[0059] Reference Figure 1 to Figure 2 As shown, Figure 1 The uncured film has a large number of voids, which will limit the transport of lithium ions and affect battery performance. As expected, the tensile strength of the electrolyte membrane is poor. Figure 2It can be seen that the pores of the cured electrolyte membrane are completely filled with the polymer precursor, which is a good conductor of lithium ions and is conducive to the transmission of lithium ions. After the polymer is cured in situ, a three-dimensional network structure is formed, which can improve the tensile strength of the solid electrolyte film.
[0060] To achieve the third objective of the present invention, an embodiment of the present invention provides a lithium-ion battery, comprising: a positive electrode active material, a negative electrode active material, and a solid electrolyte membrane as described in any of the above embodiments.
[0061] The lithium ion battery of this embodiment includes the solid electrolyte membrane of any embodiment of the present invention, and thus has all the beneficial effects of the solid electrolyte membrane of any embodiment of the present invention, which will not be described in detail here. Example 1
[0062] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0063] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=600), lithium bis(oxalatoborate) and AIBN were added in order according to 50:10:22:2 parts by weight, and stirred evenly to obtain a polymer precursor;
[0064] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 1 μm, heating at 80° C., and curing for 24 hours to obtain a solid electrolyte membrane. Example 2
[0065] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0066] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=900), lithium bis(oxalatoborate) and AIBN were added in order according to 50:10:22:2 parts by weight, and stirred evenly to obtain a polymer precursor;
[0067] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the thickness of the polymer precursor is controlled at 2 μm, heating at 80° C., and curing for 24 hours to obtain a solid electrolyte membrane. Example 3
[0068] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0069] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=1500), lithium bis(oxalatoborate) and AIBN were added in order according to 50:10:22:2 parts by weight, and stirred evenly to obtain a polymer precursor;
[0070] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the thickness of the polymer precursor is controlled at 5 μm, heating at 80° C., and curing for 24 hours to obtain a solid electrolyte membrane. Example 4
[0071] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0072] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=900), lithium bis(oxalatoborate) and AIBN were added in order according to 50:10:22:2 parts by weight, and stirred evenly to obtain a polymer precursor;
[0073] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 0.5 μm, heating at 80° C., and curing for 24 hours to obtain a solid electrolyte membrane. Example 5
[0074] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0075] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=900), lithium bis(oxalatoborate) and AIBN were added in order according to 50:10:22:2 parts by weight, and stirred evenly to obtain a polymer precursor;
[0076] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 7 μm, heating at 80° C., and curing for 24 hours to obtain a solid electrolyte membrane. Example 6
[0077] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 1000:5, and rolling them into a film at 100° C. to obtain an electrolyte layer;
[0078] S200, under an inert gas protective atmosphere, LiAsF6, PEGDA (MW=1500), lithium bis(oxalatoborate) and dimethyl azobis(isobutyrate) are added in sequence according to 55:13:20:4 parts by weight, and stirred evenly to obtain a polymer precursor;
[0079] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 2 μm, heating at 80° C., heating at 70° C., and curing for 12 hours to obtain a solid electrolyte membrane. Example 7
[0080] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 100:8, and rolling them into a film at 120° C. to obtain an electrolyte layer;
[0081] S200, under an inert gas protective atmosphere, LiBF6, tripropylene glycol diacrylate (MW=800), lithium difluorooxalatoborate and AIBN are added in sequence according to 57:18:22:2 parts by mass, and stirred evenly to obtain a polymer precursor;
[0082] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 2 μm, heating at 80° C., and curing for 12 hours to obtain a solid electrolyte membrane. Example 8
[0083] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 10:1, and rolling them into a film at 100° C. to obtain an electrolyte layer;
[0084] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, tri(ethylene glycol) diacrylate (MW=1400), lithium difluorooxalatoborate and benzoyl peroxide are added in sequence according to 60:15:25:3 parts by weight, and stirred evenly to obtain a polymer precursor;
[0085] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the thickness of the polymer precursor is controlled at 2 μm, heating at 50° C., and curing for 48 hours to obtain a solid electrolyte membrane. Example 9
[0086] S100, in an inert gas protective atmosphere, grinding and mixing a sulfide solid electrolyte and a PTFE binder at a mass ratio of 1000:1, and rolling them into a film at 80° C. to obtain an electrolyte layer;
[0087] S200, under an inert gas protective atmosphere, 1-vinyl-3-butylimidazole bis-(trifluoromethylsulfonyl)imide, PEGDA (MW=1200), LiTFSi and AIBN were added in order according to 55:20:30:4 parts by mass, and stirred evenly to obtain a polymer precursor;
[0088] S300, coating the polymer precursor on the electrolyte layer, controlling the coating thickness so that the polymer precursor thickness is controlled at 2 μm, heating at 75° C., and curing for 24 hours to obtain a solid electrolyte membrane.
[0089] Comparative Example 1
[0090] Under an inert gas protective atmosphere, a sulfide solid electrolyte and a PTFE binder were ground and mixed uniformly at a mass ratio of 100:1, and then rolled into a film at 80°C to obtain a solid electrolyte membrane.
[0091] Comparative Example 2
[0092] The preparation method of this embodiment is similar to that of the second embodiment, except that non-woven fabric is added in S200.
[0093] Comparative Example 3
[0094] Under an inert gas protective atmosphere, the sulfide solid electrolyte is directly pressed into a film.
[0095] Performance Testing
[0096] The solid electrolyte membrane of the embodiment of the present application can be prepared into a battery material according to the following method:
[0097] Under an inert gas protective atmosphere, the ternary cathode material, sulfide solid electrolyte, PTFE binder and conductive carbon were weighed in a mass ratio of 70:30:1:3, ground and mixed evenly, and then repeatedly rolled at 100°C using a roller press to obtain a cathode;
[0098] Under an inert gas protective atmosphere, a graphite negative electrode material, a sulfide solid electrolyte, and a PTFE binder are weighed in a mass ratio of 70:30:1:3, ground and mixed evenly, and then repeatedly rolled at 100° C. using a roller press to obtain a negative electrode;
[0099] The negative electrode, solid electrolyte membrane and positive electrode are placed in an assembly device in sequence and pressurized to produce a lithium-ion battery.
[0100] Table 1
[0101] According to the performance test results in Table 1, it can be seen that in Examples 1 to 5 of the present application, the tensile strength of the battery material is improved because the solid electrolyte membrane includes a polymer precursor layer. However, since the polymer precursor layer can conduct lithium ions, its lithium ion conductivity is not as good as that of the sulfide solid electrolyte. Therefore, if the coating thickness of the polymer precursor layer is too thin, it will not be able to effectively isolate the PTFE and the negative electrode, resulting in a decrease in the capacity retention rate. If the coating thickness is too thick, the lithium ion transmission will be limited, thereby resulting in a decrease in the capacity retention rate. The solid electrolyte membrane of Comparative Example 1 lacks a mechanical support layer, resulting in poor tensile strength, and there is no polymer precursor layer to isolate PTFE from the negative electrode, which will cause PTFE to be reduced to a carbon conductive network, thereby causing a battery short circuit; According to Example 2 and Comparative Example 2, it can be seen that when the solid electrolyte membrane has a polymer precursor layer, the non-woven fabric material is added at the same time, which increases the tensile strength of the battery material, but the addition of the poor conductor of the non-woven fabric has an adverse effect on the capacity retention rate of the battery material; Comparative Example 3 adopts a tabletting method to obtain a battery material, which has a good capacity retention rate, but it is not flexible, which not only makes it difficult to enlarge and manufacture, but also greatly reduces the energy density of the resulting battery.
[0102] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0103] In this specification, the writing method of "S100", "S200" and "S300" is to facilitate the description of the embodiments of the present invention. The present invention can also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited by the order of the specific embodiments of the above writing method.
[0104] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A solid electrolyte membrane, It is characterized in that The solid electrolyte membrane comprises: An electrolyte layer, the electrolyte layer comprising a sulfide and a PTFE binder; A polymer precursor layer, the polymer precursor layer is arranged near the negative electrode active material side, the polymer precursor layer is formed after the polymer precursor is cured, and the polymer precursor includes a polyene polymer; The thickness of the polymer precursor layer is 1 μm-5 μm; The molecular weight of the polyene polymer is 600-1500; The polyolefin polymer includes at least one of PEGDA, tripropylene glycol diacrylate and tri(ethylene glycol) diacrylate.
2. The solid electrolyte membrane according to claim 1, It is characterized in that The polymer precursor comprises, in parts by mass: Ionic liquid, 50 to 60 parts by mass; Polyene polymer, 10-20 parts by mass; Lithium salt, 20-30 parts by mass; Initiator: 2 to 4 parts by mass.
3. The solid electrolyte membrane according to claim 2, It is characterized in that The ionic liquid includes: 1-vinyl-3-butyl imidazole bis-(trifluoromethylsulfonyl) imide, LiAsF 6 、LiPF 6 , LiBF 6 、LiClO 4 At least one of; and / or The lithium salt comprises: at least one of LiTFSi, lithium bis(oxalatoborate), and lithium difluorooxalatoborate; and / or The initiator comprises at least one of AIBN, dimethyl azobisisobutyrate and benzoyl peroxide.
4. A method for preparing a solid electrolyte membrane according to any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: S100, in an inert gas protective atmosphere, grinding and mixing the sulfide and the PTFE binder evenly, and rolling them into a film to obtain the electrolyte layer; S200, preparing the polymer precursor under an inert gas protective atmosphere; S300, coating the polymer precursor on the electrolyte layer, and heating and curing the layer to obtain the solid electrolyte membrane.
5. The preparation method according to claim 4, It is characterized in that In S100, the amount of the PTFE binder added is 0.1%-10% of the sulfide; and / or In S100, the temperature of the rolling is 50°C-150°C.
6. The preparation method according to claim 4, It is characterized in that S200 specifically includes: Under an inert gas protective atmosphere, the ionic liquid, the polyene polymer, the lithium salt and the initiator are added in order according to parts by mass and stirred evenly to obtain the polymer precursor.
7. The preparation method according to claim 4, It is characterized in that In S300, the temperature of the heating and curing is 50°C-80°C; and / or In S300, the heating and curing time is 12h-48h.
8. A lithium ion battery, It is characterized in that include: A positive electrode active material, a negative electrode active material, and a solid electrolyte membrane as claimed in any one of claims 1 to 3.