A method for preparing a high-voltage solid polymer lithium metal battery

By preparing a high-voltage resistant polymer protective layer and a high-voltage solid electrolyte in situ on the lithium metal surface, the problem of instability of lithium metal batteries under high voltage was solved, and battery stability under high voltage and high voltage was achieved, with high initial discharge capacity and good cycle performance.

CN118017020BActive Publication Date: 2024-11-26SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410390183.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-11-26
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

Existing lithium metal batteries require an oxygen-free and water-free environment during the manufacturing process, resulting in high costs. At the same time, commonly used polymer electrolytes are unstable at high voltages and are prone to side reactions with lithium metal. Furthermore, the modification process is complex and difficult to mass-produce.

Method used

A protective layer is prepared in situ on the lithium metal surface using a high-voltage resistant polymer electrolyte and a lithium metal-stabilized polymer. This forms a lithium metal protective layer that isolates the lithium metal from the corrosion of oxygen and water in the air and prevents harmful chemical reagents from corroding the lithium metal under high voltage. At the same time, a solid polymer electrolyte capable of withstanding high voltage is prepared on the positive electrode.

Benefits of technology

It has made it feasible to assemble lithium metal batteries in air, ensuring lithium-ion conduction, preventing chemical reagent corrosion, and maintaining stable battery operation at high voltage, exhibiting high initial discharge specific capacity, reliable cycle and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118017020B_ABST
    Figure CN118017020B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of lithium metal batteries, and discloses a method for preparing a high-voltage resistant solid polymer lithium metal battery. The preparation method of the present invention comprises in-situ forming a high-voltage resistant polymer electrolyte and a polymer lithium metal protective layer on a high-voltage positive electrode and a lithium metal negative electrode, respectively. Among them, the high-voltage resistant polymer electrolyte on the high-voltage positive electrode can ensure that the battery operates stably under high-potential conditions; the polymer protective layer on the lithium metal electrode can ensure that the battery is protected from oxygen, water and other substances that may react with lithium metal during the assembly process in the air, and can also ensure that the lithium metal is protected from corrosion from organic substances in the electrolyte or electrolyte during the operation of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium metal batteries, and in particular to a method for preparing a high-voltage resistant solid polymer lithium metal battery. Background Art

[0002] Currently, due to the active chemical properties of lithium metal, the assembly process of lithium metal batteries needs to be carried out in an oxygen-free and water-free environment. This high environmental requirement greatly increases the cost of battery preparation. The polymer protective layer on the lithium metal electrode can ensure that the lithium metal is protected from oxygen, water and other substances that may react with lithium metal during the assembly process of the battery in the air, but there are also some problems with high-voltage polymer solid-state lithium metal batteries. First, polymer electrolytes that can withstand high voltages usually have some residual organic solvents during preparation. These organic solvents promote the rapid conduction of lithium ions in the polymer on the one hand, but on the other hand, they face the problem of side reactions with the lithium metal negative electrode that damage the health of the battery. Second, commonly used polymer electrolytes can not damage lithium metal when in contact with lithium metal, but have the disadvantage of being difficult to withstand stable operation of the battery at higher voltages.

[0003] There is currently no good solution to the first problem mentioned above. For the second problem, there are currently two main solutions: one is to strictly control the content of chemical solvents that are unstable to metals in high-voltage polymer electrolytes or to limit the diffusion of chemical solvents through special means; the other is to modify the commonly used polymer electrolytes. Although this method has improved the high-voltage resistance of the electrolyte to a certain extent, the process is relatively complicated and costly, and it remains in the laboratory stage and is difficult to mass produce. Therefore, a method is needed to solve the above problems at the same time. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned background technology, use a high-voltage resistant polymer electrolyte and a lithium metal stable polymer to effectively solve the above-mentioned problems, and provide a method for preparing a high-voltage resistant solid polymer lithium metal battery. The preparation method uses a simple physical method to prepare a polymer electrolyte that is stable to lithium metal in situ on the surface of lithium metal to form a lithium metal protective layer, so that it can isolate the corrosion of lithium metal by oxygen and water in the air during assembly, and at the same time, it can ensure the shuttle of lithium ions when the battery is running, and prevent the corrosion of lithium metal by chemical reagents harmful to lithium metal in the electrolyte, and the solid polymer electrolyte that can withstand high voltage prepared on the high-voltage positive electrode ensures the stable operation of the battery at high voltage.

[0005] To achieve the purpose of the present invention, the preparation method of the high voltage resistant solid polymer lithium metal battery of the present invention comprises:

[0006] (1) dissolving a high voltage resistant polymer in an organic solvent to prepare a polymer solution of a certain concentration, adding lithium salt and inorganic nanoparticles for improving lithium ion conductivity to the solution and stirring the solution to form a solid polymer electrolyte solution;

[0007] (2) dissolving the lithium metal protective layer polymer in an organic solvent to prepare a polymer solution of a certain concentration, adding a lithium salt that improves lithium ion conductivity to the solution and stirring evenly to form a negative electrode protective layer solution;

[0008] (3) directly coating the solid polymer electrolyte solution on the positive electrode and drying it to form a solid polymer electrolyte, thereby obtaining a positive electrode with a high-voltage resistant polymer electrolyte, the thickness of which is adjusted according to actual needs, which can be achieved specifically by coating thickness;

[0009] (4) directly coating the negative electrode protective layer solution on the lithium metal cut into the required size and drying it to form a lithium metal protective layer, thereby obtaining a lithium metal negative electrode with a protective layer, the thickness of which is adjusted according to actual needs;

[0010] (5) The positive electrode with the high-voltage polymer electrolyte and the lithium metal negative electrode with the protective layer obtained above are assembled in a conventional manner. Since there is a protective layer on the surface of the lithium metal, the environment during battery assembly is not restricted.

[0011] Furthermore, in some embodiments of the present invention, the high voltage resistant polymer in step (1) is one or more of a fluorine-containing polymer, a cyanide-containing polymer, polycaprolactone (PCL), and polyoxalate (POE); preferably, the fluorine-containing polymer is polyvinyl fluoride (PVF) or polyvinylidene fluoride (PVDF); preferably, the cyanide-containing polymer is polycyanoacrylate or ethyl cyanoacrylate (ECA); more preferably, the high voltage resistant polymer in step (1) is polyvinylidene fluoride (PVDF).

[0012] Furthermore, in some embodiments of the present invention, the lithium metal protective layer polymer in step (2) is one or more of a chlorine-containing polymer, an ether polymer, and polysiloxane (PS); preferably, the chlorine-containing polymer is one or more of polyvinyl chloride (PVC) and polyvinylidene chloride (PVDC); preferably, the ether polymer is one or more of polyethylene oxide (PEO), ethylene glycol methyl ether methacrylate (PEGMA), and polydioxolane (P-DOL); more preferably, the lithium metal protective layer polymer in step (2) is polyvinylidene chloride (PVDC).

[0013] Furthermore, in some embodiments of the present invention, the lithium salt in step (1) and step (2) is one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluorosulfonylimide), and lithium bis(trifluoromethylsulfonylimide).

[0014] Furthermore, in some embodiments of the present invention, the inorganic nanoparticles in step (1) are silicon dioxide, zirconium oxide, titanium dioxide, Li 7 La 3 Zr 2 O 12 , Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , Li 10 G 2 S 12 , Li 6 PS 5 One or more of Cl.

[0015] Furthermore, in some embodiments of the present invention, in step (1), the mass ratio of the high voltage resistant polymer, the lithium salt, and the inorganic nanoparticles is 40-70:5-40:5-30.

[0016] Different polymers in the preparation method of the present invention have corresponding solvents for dissolving. Researchers in the field can choose according to the physical property information. For the preferred polyvinylidene fluoride (PVDF) in step (1) of the above preparation method, the preferred solvents are N, N-dimethylformamide (DMF) and N, N-dimethylacetamide (DMAc); for the preferred polyvinylidene chloride (PVDC) in step (2) of the above preparation method, the preferred solvents are tetrahydrofuran (THF) and dichloromethane (DCM).

[0017] Furthermore, in some embodiments of the present invention, the organic solvent used in step (1) is a poor solvent for the lithium metal protective layer polymer in step (2), and the organic solvent used in step (2) is a poor solvent for the high voltage resistant polymer in step (1).

[0018] Furthermore, in some embodiments of the present invention, the solvent content in the solid polymer electrolyte solution in step (1) is 5-10% to promote lithium ion conduction.

[0019] Furthermore, in some embodiments of the present invention, the solvent content in the negative electrode protective layer solution in step (2) is 5-10% to promote lithium ion conduction.

[0020] Furthermore, in some embodiments of the present invention, the preparation of the lithium metal protective layer in step (4) is carried out in a glove box filled with inert gas, and the water and oxygen values ​​in the glove box should be less than 0.1 ppm.

[0021] Furthermore, in some embodiments of the present invention, in step (5), an electrolyte needs to be added between the high voltage resistant polymer and the lithium metal protection layer polymer for wetting during assembly.

[0022] Compared with the prior art, the advantages of the present invention are as follows:

[0023] (1) The use of a high-voltage stable polymer substrate at the cathode / electrolyte interface in the present invention can better match the high-voltage cathode.

[0024] (2) The use of a lithium metal stabilizing polymer at the lithium metal negative electrode / electrolyte interface in the present invention can effectively prevent lithium metal from being corroded by moist air and organic solvents, thereby achieving chemical stability of the lithium metal electrode. Therefore, the composite electrolyte has a wide electrochemical stability window and excellent positive electrode interface stability.

[0025] (3) In practical applications, the technology of the present invention can be used as a solid electrolyte for high energy density lithium metal batteries, while meeting the requirements for the assembly of lithium metal batteries in air. The prepared high-voltage solid-state lithium metal batteries exhibit high initial discharge specific capacity, reliable cycle and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the performance of the battery obtained in Example 1 of the present invention during long-term charge and discharge cycles;

[0027] Figure 2 Schematic diagram of the performance of the battery obtained in Example 2 of the present invention during long-term charge and discharge cycles;

[0028] Figure 3 Schematic diagram of the performance of the battery obtained in Comparative Example 1 of the present invention after long-term charge and discharge cycles;

[0029] Figure 4 It is a performance diagram of the battery obtained in comparative example 2 of the present invention subjected to long-term charge and discharge cycles. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Additional aspects and advantages of the present invention will be partially given in the following description, partially become apparent from the following description, or be understood through the practice of the present invention. It should be understood that the following description is only used to explain the present invention and is not intended to limit the present invention.

[0031] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0032] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0033] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0034] In addition, the descriptions of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described below mean that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the technical features involved in the various embodiments of the present invention can be combined with each other as long as they do not conflict with each other. Example 1

[0035] A method for preparing a high-voltage solid-state polymer lithium metal battery comprises the following steps:

[0036] 1. Polyvinylidene fluoride (PVDF), lithium bis(difluorosulfonyl)imide (LiTFSI), Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 Add the mixture into 15 mL of N,N-dimethylformamide (DMF) organic solvent in a mass ratio of 0.6 g: 0.1 g: 0.3 g and stir overnight to dissolve the mixture to obtain a PVDF polymer electrolyte solution;

[0037] 2. Add polyvinylidene chloride (PVDC) and lithium bis(difluorosulfonyl)imide (LiTFSI) in a mass ratio of 1.0 g:0.4 g into 15 mL of tetrahydrofuran (THF) organic solvent and stir for one day and night to dissolve to obtain a PVDC polymer solution;

[0038] 3. 100 μl of the PVDF polymer electrolyte solution obtained in step 1 was drop-coated on a 12 mm diameter NCM811 positive electrode, and then volatilized for 24 h to obtain a polymer electrolyte;

[0039] 4. In a glove box where the water and oxygen concentrations are both less than 0.1 ppm, 175 μl of the PVDC polymer solution obtained in step 2 is drop-coated on a lithium metal sheet with a diameter of 18 mm, and a lithium metal protective layer is obtained after 12 hours of volatilization;

[0040] 5. After completing the above steps, the button cell can be assembled in the air according to the conventional steps. It should be noted that 15 μl of electrolyte needs to be added between the PVDC polymer and the PVDF polymer for wetting during assembly.

[0041] 6. After leaving the battery for 12 hours, perform a charge and discharge curve at a rate of 0.5C. Example 2

[0042] A method for preparing a high-voltage solid-state polymer lithium metal battery comprises the following steps:

[0043] 1. Polyvinylidene fluoride (PVDF), lithium bis(difluorosulfonyl)imide (LiTFSI), Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , adding 0.8 g:0.15 g:0.6 g into 20 mL of N, N-dimethylformamide (DMF) organic solvent and stirring overnight to dissolve to obtain a PVDF polymer electrolyte solution;

[0044] 2. Add polyvinylidene chloride (PVDC) and lithium bis(difluorosulfonyl)imide (LiTFSI) in a mass ratio of 1.5 g:0.5 g into 20 mL of tetrahydrofuran (THF) organic solvent and stir for one day and night to dissolve to obtain a PVDC polymer solution;

[0045] 3. 80 μl of the PVDF polymer electrolyte solution obtained in step 1 was drop-coated on the LCO positive electrode with a diameter of 12 mm, and then volatilized for 24 hours to obtain the polymer electrolyte;

[0046] 4. In a glove box where the water and oxygen concentrations are both less than 0.1 ppm, 155 μl of the PVDC polymer solution obtained in step 2 is drop-coated on a lithium metal sheet with a diameter of 18 mm, and a lithium metal protective layer is obtained after 12 hours of volatilization;

[0047] 5. After completing the above steps, the button cell can be assembled in the air according to the conventional steps. It should be noted that 15 μl of electrolyte needs to be added between the PVDC polymer and the PVDF polymer for wetting during assembly.

[0048] 6. After leaving the battery for 12 hours, perform a charge and discharge curve at a rate of 0.1C. Example 3

[0049] A method for preparing a high-voltage solid-state polymer lithium metal battery comprises the following steps:

[0050] 1. Polycaprolactone (PCL), lithium hexafluorophosphate (LiPF 6 )、Li 7 La 3 Zr 2 O 12 , adding 0.3 g: 0.04 g: 0.14 g into 10 mL of N, N-dimethylformamide (DMF) organic solvent and stirring overnight to dissolve to obtain a PCL polymer electrolyte solution;

[0051] 2. Ethylene vinyl acetate (EVA), lithium hexafluorophosphate (LiPF 6 ) was added into 10 mL of tetrahydrofuran (THF) organic solvent in a mass ratio of 0.8 g:0.23 g and stirred for one day and night to dissolve to obtain an EVA polymer solution;

[0052] 3. 100 μl of the PCL polymer electrolyte solution obtained in step 1 was drop-coated on a 12 mm diameter NCM523 positive electrode, and then evaporated for 24 h to obtain a polymer electrolyte;

[0053] 4. In a glove box where the water and oxygen concentrations are both less than 0.1 ppm, 125 μl of the EVA polymer solution obtained in step 2 is drop-coated on a lithium metal sheet with a diameter of 18 mm, and a lithium metal protective layer is obtained after 12 hours of volatilization;

[0054] 5. After completing the above steps, the button cell can be assembled in the air according to the normal steps. It should be noted that 15μl of electrolyte needs to be added between the PCL polymer and the EVA polymer for wetting during assembly;

[0055] 6. After leaving the battery for 12 hours, perform the charge and discharge curve at a rate of 0.3C. Comparative Example 1

[0056] A method for preparing a lithium metal battery comprises the following steps:

[0057] 1. Polyvinylidene fluoride (PVDF), lithium bis(difluorosulfonyl)imide (LiTFSI), Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , adding 0.6 g: 0.1 g: 0.3 g into 15 mL of N, N-dimethylformamide (DMF) organic solvent and stirring overnight to dissolve to obtain a PVDF polymer electrolyte solution;

[0058] 2. 100 μl of the PVDF polymer electrolyte solution obtained in step 1 was drop-coated on a 12 mm diameter NCM811 positive electrode, and then volatilized for 24 h to obtain a polymer electrolyte;

[0059] 3. Then, in a glove box where the water and oxygen concentrations are less than 0.1 ppm, a lithium metal battery is assembled with lithium metal as the negative electrode; it should be noted that 15 μl of electrolyte is added between the electrolyte and the lithium metal for wetting;

[0060] 4. After leaving the battery for 12 hours, perform the charge and discharge curve at a rate of 0.5C. Comparative Example 2

[0061] A method for preparing a lithium metal battery comprises the following steps:

[0062] 1. Add polyvinylidene chloride (PVDC) and lithium bis(difluorosulfonyl)imide (LiTFSI) in a mass ratio of 1.0 g:0.4 g into 10 mL of tetrahydrofuran (THF) organic solvent and stir for one day and night to dissolve to obtain a PVDC polymer electrolyte solution;

[0063] 2. 200 μl of the PVDC polymer electrolyte solution obtained in step 1 was drop-coated on NCM811 with a diameter of 12 mm, and the PVDC polymer electrolyte was obtained after 12 hours of volatilization;

[0064] 3. Then, in a glove box where the water and oxygen concentrations are less than 0.1 ppm, a lithium metal battery is assembled with lithium metal as the negative electrode; it should be noted that 15 μl of electrolyte is added between the electrolyte and the lithium metal for wetting;

[0065] 4. After leaving the battery for 12 hours, perform the charge and discharge curve at a rate of 0.5C.

[0066] The performance test results of the batteries obtained in the above examples and comparative examples are shown below.

[0067] Test items Charging voltage Charge and discharge rate Specific capacity after 100 cycles (mAh / g) Capacity retention after 100 cycles (%) Example 1 4.3 0.5C 133.1 94.7 Example 2 4.3 0.1C 117.7 86.3 Example 3 4.3 0.3C 141.3 91.2 Comparative Example 1 4.3 0.5C 74.1 80.2 Comparative Example 2 4.3 0.5C 0 0

[0068] Example 1 A battery with NCM811 as the high voltage positive electrode and lithium metal as the negative electrode was subjected to a long-term charge and discharge cycle at a high current density. Figure 1 As shown, the battery has stable discharge capacity and coulombic efficiency. The capacity retention rate reaches 84.2% when cycled 200 times at a rate of 0.5C. The reversible capacity is still greater than 70% when extended to more than 300 cycles. The average coulombic efficiency in the entire cycle process is greater than 98.5%. Even after multiple charge and discharge processes, it still has almost overlapping charge and discharge curves.

[0069] Example 2 A battery with LCO as a high voltage positive electrode and lithium metal as a negative electrode was subjected to a long-term charge and discharge cycle at a high current density. Figure 2 As shown in the figure, the battery has stable discharge capacity and coulombic efficiency. The battery also has good cycle stability and a coulombic efficiency close to 100% at a current density of 0.1C. After 150 charge and discharge cycles, the capacity retention rate is still more than 80%.

[0070] like Figure 3 As shown, the battery in Comparative Example 1, which uses a high-voltage electrolyte alone and uses NCM811 as a high-voltage positive electrode and lithium metal as a negative electrode, has been subjected to a long-term charge and discharge cycle at a high current density and exhibits low capacity from the beginning.

[0071] like Figure 4 As shown, the battery in Comparative Example 2, which used ordinary electrolyte alone, with NCM811 as the high-voltage positive electrode and lithium metal as the negative electrode, was subjected to a long period of charge and discharge cycle at a high current density. It showed a particularly low capacity from the beginning, and the battery failed within 100 charge and discharge cycles.

[0072] It will be easily understood by those skilled in the art that the above descriptions are only partial embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-voltage solid-state polymer lithium metal battery, characterized in that: The method comprises: (1) dissolving a high voltage resistant polymer in an organic solvent to prepare a polymer solution of a certain concentration, adding lithium salt and inorganic nanoparticles for improving lithium ion conductivity to the solution and stirring the solution to form a solid polymer electrolyte solution; (2) dissolving the lithium metal protective layer polymer in an organic solvent to prepare a polymer solution of a certain concentration, adding a lithium salt that improves lithium ion conductivity to the solution and stirring evenly to form a negative electrode protective layer solution; (3) directly coating the solid polymer electrolyte solution on the positive electrode and drying it to form a solid polymer electrolyte, thereby obtaining a positive electrode with a high-voltage resistant polymer electrolyte, the thickness of which is adjusted according to actual needs, which can be achieved specifically by coating thickness; (4) directly coating the negative electrode protective layer solution on the lithium metal cut into the required size and drying it to form a lithium metal protective layer, thereby obtaining a lithium metal negative electrode with a protective layer, the thickness of which is adjusted according to actual needs; (5) Assembling the above-obtained positive electrode with a high-voltage polymer electrolyte and a lithium metal negative electrode with a protective layer in a conventional manner. During assembly, an electrolyte needs to be added between the high-voltage polymer and the lithium metal protective layer polymer for wetting. Since there is a protective layer on the surface of the lithium metal, the environment during battery assembly is not restricted; In the step (1), the high voltage resistant polymer is one or more of a fluorine-containing polymer, a cyanide-containing polymer, polycaprolactone (PCL), and polyoxalate (POE); the fluorine-containing polymer is one or more of polyvinyl fluoride (PVF) and polyvinylidene fluoride (PVDF); the cyanide-containing polymer is polycyanoacrylate; In the step (2), the lithium metal protective layer polymer is a chlorine-containing polymer and / or polysiloxane (PS); the chlorine-containing polymer is one or more of polyvinyl chloride (PVC) and polyvinylidene chloride (PVDC); The organic solvent used in step (1) is a poor solvent for the lithium metal protective layer polymer in step (2), and the organic solvent used in step (2) is a poor solvent for the high voltage resistant polymer in step (1); Among them, the role of the lithium metal protective layer is to isolate the lithium metal from the corrosion of oxygen and water in the air. At the same time, it can ensure the shuttling of lithium ions when the battery is running, and prevent the corrosion of lithium metal by chemical reagents harmful to lithium metal in the electrolyte.

2. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: The lithium salt in step (1) and step (2) is one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluorosulfonylimide), and lithium bis(trifluoromethylsulfonylimide).

3. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: The inorganic nanoparticles in step (1) are silicon dioxide, zirconium oxide, titanium dioxide, Li7La3Zr2O 12 , Li 6.4 LqCy 1.4 Ta 0.6 O 12 , Li 10 GeP2S 12 , Li6PS5Cl or more.

4. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: In the step (1), the mass ratio of the high voltage resistant polymer, the lithium salt and the inorganic nanoparticles is 40-70:5-40:5-30.

5. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: The solvent content in the solid polymer electrolyte solution in step (1) is 5-10% to promote lithium ion conduction.

6. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: The solvent content in the negative electrode protective layer solution in step (2) is 5-10% to promote lithium ion conduction.

7. The method for preparing a high voltage resistant solid polymer lithium metal battery according to claim 1, characterized in that: The preparation of the lithium metal protective layer in step (4) is carried out in a glove box filled with inert gas, and the water and oxygen levels in the glove box should be less than 0.1 ppm.