Film for stent graft and preparation method thereof, and stent graft

By using the integrated braiding of the basic covering area and the variable-strength covering area in the covered stent, the problem of reduced compressibility caused by overlap during suturing is solved, allowing both intracavitary and open surgery to be applied, and improving the compressibility of surgery. and suture strength.

CN118021493BActive Publication Date: 2024-10-15BEIJING PERCUTEK THERAPEUTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410197460.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-15
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

The existing covered stent requires two layers of coverings to overlap during suturing, which results in an increase in the thickness of the overlapping area and reduced compressibility. It cannot be compressed into a small-diameter delivery device, which limits the application of intraluminal surgery.

Method used

The basic coating area and the variable strength coating area are arranged at intervals along the axial direction of the coating. By adjusting the interweaving method and number of warp and weft yarns, an integrated braided reinforced seamable coating is formed to ensure stitching strength and compressibility, and is suitable for In intracavitary and open surgery.

Benefits of technology

The stent graft achieves both compressibility and suture strength, and can be compressed into a small-diameter delivery device for intraluminal surgery. It also provides stable suture strength during open surgery, reducing surgical difficulty and complications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118021493B_ABST
    Figure CN118021493B_ABST
Patent Text Reader

Abstract

The present invention discloses a coating for a stent graft, a preparation method thereof, and a stent graft. The basic coating area and the variable strength coating area are integrally woven to form an integrated reinforced sutureable coating. The weaving method of different reinforcement strengths in different regions of the fabric is achieved by adjusting the weaving method of the fabric yarn and the number of yarns. The basic coating area and the variable strength coating area are integrally woven, and no cutting, overlapping, or sewing is required. The coating area can be compressed into a small-caliber conveyor, which is more conducive to intracavitary surgical delivery and reduces the caliber of the conveyor. The variable strength coating area can be used as a suture area to directly suture with the main blood vessel, and the suture strength is guaranteed, which is convenient for in-situ sewing during open surgery, and is not easy to produce internal leakage due to holes, thereby solving the problem of difficulty in sewing during or after the existing coated stent graft. The coating for the stent graft proposed by the present invention takes into account both compressibility and suture strength, and can be used for both intracavitary surgery and in-situ suture of open surgery, and is highly practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of medical devices, and in particular to a coating for a coated stent, a preparation method thereof, and a coated stent. Background Art

[0002] In the past decade, endovascular repair has become a routine treatment for thoracic aortic aneurysms, aortic dissections, and abdominal aortic aneurysms with appropriate anatomy due to its advantages of less trauma, faster recovery, fewer perioperative complications, and low mortality. The endovascular treatment device needs to compress the stent graft into the delivery sheath, which needs to enter from the femoral artery to deliver the stent graft to the lesion site. The usual femoral artery diameter is only 6~7mm, which puts forward requirements for the diameter of the delivery sheath and the compressed volume of the stent graft. In order to meet the compression requirements, the coating thickness of the endovascular stent graft currently sold on the market is set at 0.1mm.

[0003] At present, endovascular repair is mainly used to treat lesions in areas without branch vessels. Lesions in the abdominal visceral region often involve endovascular reconstruction of multiple branch vessels, which is extremely difficult and usually requires open surgery for treatment. In addition, some patients have certain complications after descending aorta surgery, such as reverse tear type A dissection (RTAD) and stent-induced new rupture (SINE). When an intraluminal covered stent has been released in the patient's body and further open surgery is required, the artificial blood vessels and covered stents used for open surgery need to be sutured with the autologous blood vessels. However, the existing 0.1mm thick thin film has low strength and cannot be sutured directly. The doctor needs to remove the implanted covered stent first, which brings difficulties to open surgery.

[0004] In order to improve the suture strength of the coating, the existing technology often uses thicker yarns to weave the coating. While the suture strength of the coating is improved, the thickness of the coating also increases, usually reaching more than 0.3 mm. This undoubtedly limits the compression capacity of the coating and brings difficulties to the early placement of the coated stent.

[0005] Currently, there is a stent for intraoperative stents used in open surgery on the market, which is a reinforced thick sutureable coating sewn on a basic thin coating for intraoperative suturing. However, there is a problem with this technology: the overlap position of the basic thin coating and the reinforced thick sutureable coating requires two layers of coating to overlap, resulting in a higher coating thickness in the overlapping area and further reduced compressibility. This technology can only be used for open surgery and cannot be compressed into a small-caliber delivery device (such as a delivery sheath) for intracavitary surgery. Summary of the invention

[0006] The object of the present invention is to provide a coating for a coated stent and a preparation method thereof, and a coated stent, so as to solve the problem that the conventional reinforced thick sutureable coating is sewn on a basic thin coating, and the overlapping position requires two layers of coating to overlap, resulting in a higher coating thickness in the overlapping area and further reduced compressibility, so that the coated stent can only be used for open surgery and cannot be compressed into a small-caliber delivery device (such as a delivery sheath) for intracavitary surgery.

[0007] To achieve the above-mentioned purpose, the present invention provides the following scheme: The present invention provides a coating for a coating bracket, comprising a basic coating area and a variable-strength coating area arranged at intervals along the axial direction of the coating, the basic coating area and the variable-strength coating area are both formed by interweaving warp yarns and weft yarns up and down, and the basic coating area and the variable-strength coating area are woven as a whole; wherein, the total number of warp yarns in the variable-strength coating area is more than the total number of warp yarns in the basic coating area, or, the total number of weft yarns in the variable-strength coating area is more than the total number of weft yarns in the basic coating area, or, the total number of warp yarns in the variable-strength coating area is more than the total number of warp yarns in the basic coating area, and the total number of weft yarns in the variable-strength coating area is more than the total number of weft yarns in the basic coating area.

[0008] Optionally, the warp yarns and weft yarns in the basic coating area are interlaced up and down, and the intersection of any warp yarn and any weft yarn forms a cross-interlacing point; a part of the warp yarns in the variable strength coating area are interlaced up and down with all the weft yarns to form a basic area, and the remaining warp yarns are interlaced up and down with a weft yarn after floating multiple weft yarns continuously to form a stitching area, and the warp yarn part that floats multiple weft yarns continuously forms a floating long line, the warp yarns in the stitching area are alternately arranged with the warp yarns in the basic area, and the intersection of any warp yarn and any weft yarn in the variable strength coating area forms a cross-interlacing point.

[0009] Optionally, in any one of the variable strength coating areas, the warp yarns of the stitching area and the warp yarns of the base area are arranged alternately, and the floating lines of all the stitching areas are arranged flush in the warp yarn direction of the coating, or, the floating lines of all the stitching areas are arranged staggered front and back with adjacent floating lines in the warp yarn direction of the coating.

[0010] Optionally, any warp yarn and any weft yarn are polyester multifilaments with a fiber fineness of 20D-100D.

[0011] Optionally, any warp yarn and any weft yarn are polyester monofilament.

[0012] Optionally, all warp yarns are polyester monofilaments, and all weft yarns are polyester multifilaments; or, all warp yarns are polyester multifilaments, and all weft yarns are polyester monofilaments.

[0013] Optionally, any warp yarn and any weft yarn are polyester multifilaments with a fiber fineness of 20D-100D, and the fiber fineness of any weft yarn in the variable-strength coating area is greater than the fiber fineness of any weft yarn in the basic coating area.

[0014] Optionally, the coating is cylindrical or truncated cone-shaped.

[0015] Optionally, any of the floating long lines floats continuously over three or more weft yarns.

[0016] Optionally, the weft yarns of the basic coating area and the variable strength coating area are arranged at the same interval, and any warp yarns in the variable strength coating area located in the basic area extend to the basic coating area, and the warp yarns of the basic coating area are interlaced with the weft yarns of the basic coating area one above and one below; in the variable strength coating area, the stitching area is provided between any adjacent basic areas, and the warp yarns of the stitching area only extend to the junction of the basic coating area and the variable strength coating area, and in the basic coating area, at the position corresponding to the warp yarns in the stitching area, no warp yarns are interlaced with weft yarns.

[0017] The present invention also proposes a method for preparing the above-mentioned coating for the coated stent, weaving the basic coating area and the variable strength coating area as a whole, including: interlacing a part of the warp yarns of the variable strength coating area with all the weft yarns up and down to form a basic area, and interlacing the remaining part of the warp yarns with a weft yarn up and down to form a stitching area after multiple weft yarns float continuously, so that the warp yarn part with multiple weft yarns float continuously forms a floating long line; using part of the warp yarns of the variable strength coating area to interlace the weft yarns of the basic coating area up and down, and cutting off the remaining part of the warp yarns of the variable strength coating area at the boundary between the variable strength coating area and the basic coating area, so that in the basic coating area, at the position corresponding to the warp yarn in the stitching area, no warp yarn is interlaced with the weft yarn.

[0018] The present invention further proposes a stent graft, comprising a corrugated stent and any one of the above-mentioned coatings for the stent graft, wherein a plurality of circles of the corrugated stent are arranged at intervals along the axial direction of the coating outside the basic coating area of ​​the coating.

[0019] Optionally, the variable strength coating area is provided at least one of the first position, the second position and the third position of the coating, wherein the first position is the proximal end of the coating, the second position is the distal end of the coating, and the third position is any position between the proximal end and the distal end of the coating.

[0020] Optionally, the corrugated bracket is provided outside the variable strength coating area located at the first position and / or the second position, and the corrugated bracket located at the variable strength coating area is not greater than the corresponding value of the corrugated bracket located at the basic coating area in at least one of the bracket wire diameter, the number of wave peaks and the amplitude.

[0021] Compared with the prior art, the present invention has achieved the following technical effects: the coating for the stent graft and the preparation method thereof proposed in the present invention, by weaving the basic coating area and the variable strength coating area as a whole, form an integrated reinforced and sutureable coating, by adjusting the weaving method of the fabric yarn and the number of warp yarns, a weaving method with different strengths in different regions of the fabric is achieved, the basic coating area and the variable strength coating area are woven as a whole, without cutting, overlapping and sewing, and can be compressed into a small-caliber conveyor (such as a conveying sheath) for intracavitary surgery, and is more conducive to intracavitary surgical delivery and reduces the diameter of the conveyor; by having the total number of warp yarns in the variable strength coating area being more than that in the basic coating area The total number of warp yarns in the membrane area, or the total number of weft yarns in the variable-strength coating area is greater than the total number of weft yarns in the basic coating area, or the total number of warp yarns and the total number of weft yarns in the variable-strength coating area are both greater than the total number of warp yarns and the total number of weft yarns in the basic coating area, which can make the fabric strength formed by the variable-strength coating area higher than that of the basic coating area. The variable-strength coating area can be used as a suture area to directly suture with the main blood vessel, and the suture strength is guaranteed, which is convenient for in-situ sewing during open surgery, and is not easy to cause internal leakage due to holes, solving the problem of difficult sewing during or after surgery of the existing coated stent; at the same time, although the suture strength of the basic coating area is relatively low, the compressibility of the coating is maintained. It can be seen that the coating for the coated stent proposed by the present invention takes into account both compressibility and suture strength, and can be used for both intracavitary surgery and in-situ suture of open surgery, and is highly practical.

[0022] In some technical schemes disclosed in the present invention, by forming floating length lines on the variable-strength coating area that can be used as a suture area, the interlacing points of some warp yarns and weft yarns can be reduced while ensuring the suture strength of the fabric in the variable-strength coating area, thereby forming a soft fabric area (i.e., the suture area) that is easy for needle and thread to be threaded, so that the variable-strength coating area has both high structural strength and easy threading characteristics, which reduces the difficulty of suture while ensuring the suture strength, and is beneficial to improving the suture effect and surgical efficiency.

[0023] The coated stent proposed in the present invention includes the above-mentioned coating for the coated stent, so that the coated stent has both compressibility and suturing strength, can be used for intracavitary surgery, and can also be used for in situ suturing of open surgery, and has strong practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 It is a schematic diagram of the structure of the coating for the coated stent disclosed in the first embodiment of the present invention.

[0026] Figure 2 This is a schematic diagram of the application of the coated stent disclosed in Example 3 of the present invention.

[0027] Figure 3 It is a schematic diagram of the structure of the coated stent disclosed in the fourth embodiment of the present invention.

[0028] Figure 4 This is a schematic diagram of the structure of the coated stent disclosed in Example 5 of the present invention.

[0029] Figure 5 This is a schematic diagram of the structure of the coated stent disclosed in Example 6 of the present invention.

[0030] Among them, the figure markings are: 100, coated stent; 1, coating for coated stent; 11, basic coating area; 12, variable strength coating area; 121, basic area; 122, suture area; 123, floating length line; 2, corrugated stent. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] One of the purposes of the present invention is to provide a coating for a coated stent to solve the problem that the existing reinforced thick sutureable coating is sewn on the basic thin coating, and the two layers of coating need to overlap at the overlapping position, resulting in a higher coating thickness in the overlapping area and further reduced compressibility, so that the coated stent can only be used for open surgery and cannot be compressed into a small-caliber delivery device (such as a delivery sheath) for intracavitary surgery.

[0033] Another object of the present invention is to provide a method for preparing the above-mentioned coating for the coated stent.

[0034] Another object of the present invention is to provide a coated stent having the above-mentioned coating.

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0036] Embodiment 1.

[0037] like Figure 1 As shown, this embodiment provides a coating 1 for a coated stent, comprising a basic coating area 11 and a variable strength coating area 12 arranged at intervals along the axial direction of the coating, the basic coating area 11 and the variable strength coating area 12 are both woven up and down by warp yarns and weft yarns, and the basic coating area 11 and the variable strength coating area 12 are woven as a whole. Among them, the total number of warp yarns in the variable strength coating area 12 is greater than the total number of warp yarns in the basic coating area 11, or the total number of weft yarns in the variable strength coating area 12 is greater than the total number of weft yarns in the basic coating area 11, or the total number of warp yarns and the total number of weft yarns in the variable strength coating area 12 are respectively greater than the total number of warp yarns and the total number of weft yarns in the basic coating area 11. By setting the number of yarns in the variable strength coating area 12 (the total number of warp yarns and / or the total number of weft yarns) to be greater than the number of yarns in the basic coating area 11 (the total number of warp yarns and / or the total number of weft yarns), the thickness of the variable strength coating area 12 formed can be thicker than the thickness of the basic coating area 11, and the strength of the corresponding variable strength coating area 12 is also higher than the strength of the basic coating area 11, thereby forming a woven body with different strengths in different regions of the fabric, wherein the variable strength coating area 12 can be used as a suture area to directly suture with the main body blood vessel, the suture strength is guaranteed, and it is convenient to sew in situ during open surgery, and it is not easy to cause internal leakage due to holes, which solves the problem of difficult sewing during or after surgery of the existing coated stent; at the same time, although the suture strength of the basic coating area 11 is relatively low, the compressibility of the coating is maintained. It can be seen that the coating 1 for the coated stent proposed by the present invention takes into account both compressibility and suture strength, and can be used for both intracavitary surgery and in situ suture of open surgery.

[0038] Furthermore, in the present embodiment, in the preferred basic coating area 11, the warp yarns and the weft yarns are interlaced up and down, and a cross interlacing point is formed at the intersection of any warp yarn and any weft yarn; in the variable strength coating area 12, a part of the warp yarns are interlaced up and down with all the weft yarns to form a basic area 121, and the remaining part of the warp yarns are interlaced up and down with a weft yarn after floating multiple weft yarns continuously to form a stitching area 122, and the warp yarn part that floats multiple weft yarns continuously forms a floating line 123. Compared with the method of interlacing the warp yarns and the weft yarns up and down, the formation of the floating line 123 reduces the interlacing points of some warp yarns and weft yarns, thereby forming a soft fabric area (i.e., the stitching area) that is easy for needle and thread threading, so that the variable strength coating area has both high structural strength and easy threading characteristics, while ensuring the stitching strength. Reduce the difficulty of stitching, and facilitate the stitching needle and thread threading. In the variable strength coating area 12, the warp yarns of the suture area 122 and the warp yarns of the base area 121 are arranged alternately, specifically: at least one warp yarn of the base area 121 is arranged for every multiple warp yarns of the suture area 122, or at least one warp yarn of the base area 121 is arranged for every one warp yarn of the suture area 122, and the intersection of any warp yarn and any weft yarn in the variable strength coating area 12 also forms a cross intersection point. In general, any warp yarn of the base coating area 11 and the variable strength coating area 12 is parallel to the axial direction of the coated stent 100, any weft yarn is perpendicular to the axial direction of the coated stent 100, and any weft yarn is arranged in a ring shape along the circumference of the coated stent 100. Figure 1 The unfolded state of the stent graft 1 used in this embodiment, wherein any warp yarn is arranged longitudinally, and any weft yarn is perpendicular to the warp yarn and arranged horizontally. It should be noted that: Figure 1 This is only a schematic diagram. In order to clearly describe the weaving structure of the yarn, the yarn fineness and the spacing between the yarns are enlarged for illustration. It does not mean that the actual distance and gap between the yarns are the size shown in the figure. Accordingly, in order to clearly show the floating length line 123, Figure 1 The shape of the floating yarn 123 is filled in, and the color of the actual floating yarn 123 is consistent with that of other warp yarns and weft yarns.

[0039] The above-mentioned coating 1 for stent grafts generally adopts a method in which part or all of the warp yarns in the basic coating area 11 are used in the warp yarns of the variable strength coating area 12 to realize the integral weaving of the basic coating area 11 and the variable strength coating area 12, thereby forming an integral reinforced and sutureable coating, and by adjusting the weaving method of the fabric yarns and the number of warp yarns used, a weaving method with different reinforcement strengths in different regions of the fabric is realized. Generally, it is preferred to adopt a method in which the total number of warp yarns in the variable strength coating area 12 is greater than the total number of warp yarns in the basic coating area 11. The basic coating area 11 and the variable strength coating area 12 are integrally woven, and do not require overlapping sewing. They can be compressed into a small-caliber conveyor (such as a conveying sheath tube) for intracavitary surgery. The variable strength coating area 12 can be used as a suture area to directly suture with the main blood vessel, and the suture strength is guaranteed, which is convenient for in-situ sewing during open surgery, and is not easy to cause internal leakage, solving the problem of difficult sewing during or after surgery of the existing coated stent grafts. It can be seen that the coating 1 for the coated stent proposed in the present technical solution takes into account both compressibility and suture strength, and can be used for both intracavitary surgery and in situ suturing in open surgery, and is highly practical.

[0040] In this embodiment, the warp yarns and weft yarns of the basic coating area 11 can be interlaced one above and one below, or one warp yarn can float over multiple weft yarns from above or below and then interlace with the next weft yarn. Generally, it is preferred to interlace the warp yarns and weft yarns one above and one below.

[0041] In the present embodiment, in any variable strength coating area 12, the warp yarns of the suture area 122 and the warp yarns of the base area 121 are preferably evenly spaced at intervals, for example, one warp yarn of the base area 121 is provided for every one warp yarn of the suture area 122, and in the entire variable strength coating area 12, all the warp yarns are preferably evenly spaced in parallel. In general, in order to ensure uniform strength, it is preferred that all the floating lines 123 in the same variable strength coating area 12 have the same length, that is, the number of weft yarns floated by each floating line 123 is the same. Based on this, the floating lines 123 of all suture areas 122 can be located at the same position in the axial direction of the coated support 100, that is, both ends of the length direction of the floating lines 123 are aligned; in addition, the floating lines 123 of all suture areas 122 can also be staggered front to back in the axial direction of the coated support 100, that is, the interweaving points of the floating lines 123 of all suture areas are all staggered front to back with the interweaving points of the adjacent floating lines 123 in the warp direction of the coating, as shown in FIG. Figure 1 As shown, the length directions of two floating lines 123 separated by one or more floating lines 123 are aligned, the length directions of the remaining floating lines 123 are aligned, and the length directions of two parts of the floating lines 123 are not aligned.

[0042] In this embodiment, any warp yarn and any weft yarn are polyester multifilaments with a fiber fineness of 20D-100D; or, any warp yarn and any weft yarn are polyester monofilaments; or, all warp yarns are polyester monofilaments and all weft yarns are polyester multifilaments; or, all warp yarns are polyester multifilaments and all weft yarns are polyester monofilaments. As a preferred embodiment, any warp yarn and any weft yarn in this embodiment are polyester multifilaments with a fiber fineness of 20D-100D. In any warp yarn and any weft yarn, the fiber fineness of the polyester multifilament can be completely the same or not completely the same. Different regions can be woven with yarns of different fiber finenesses, so that the woven thickness of different coated regions can be different. In the coating 1 for the coated stent of the present embodiment, whether it is the basic coating area 11 or the variable strength coating area 12, as long as there is a requirement for variable thickness, the warp yarns or weft yarns with different fiber finenesses can be replaced at the corresponding positions for weaving to achieve variable thickness of the coating. Generally, the larger the fiber fineness value, the thicker the weft yarns and warp yarns, and the thicker the coating area formed by weaving, and vice versa. For example, under the premise of exactly the same weaving interlacing method, the coating thickness formed by weaving polyester multifilament with a fiber fineness of 50D is greater than the coating thickness formed by weaving polyester multifilament with a fiber fineness of 30D.

[0043] In this embodiment, it is preferred that the fiber fineness of any weft yarn in the variable strength coating area 12 is not less than the fiber fineness of any weft yarn in the basic coating area 11. For example, the variable strength coating area 12 uses yarn with a fiber fineness of 100D as weft yarn, and the basic coating area 11 can use yarn with a fiber fineness of 50D as weft yarn; the fiber fineness of any warp yarn is not less than the fiber fineness of any warp yarn in the basic coating area 11.

[0044] In this embodiment, the coating 1 used for the stent graft is tubular as a whole, specifically cylindrical or truncated cone. When the coating is cylindrical, it is a uniform structure, and the diameter of any cross section in the axial direction is basically the same; when the coating is truncated cone, the whole is axially large at one end and small at the other end, which is a variable diameter structure. Considering that the lesion site of the blood vessel is generally large at one end and small at the other end, setting the coating in a truncated cone shape can better adapt to the morphology of the autologous blood vessels, fit well with the autologous blood vessels, and improve the treatment effect. When the coating 1 of the stent graft is set to a variable diameter truncated cone, the coating diameter reduction can be achieved by not interweaving the warp yarns at the corresponding position. The non-interwoven warp yarns are generally located on both sides of the coating. After the coating is woven, the non-interwoven warp yarns can be cut off on the coating using tools such as scissors.

[0045] In this embodiment, it is preferred that any floating line 123 floats over three or more weft yarns continuously.

[0046] In this embodiment, the unfolded shape of the variable strength coating area 12 is various, and can be a rectangle, a trapezoid, an ellipse or other shapes. Taking a rectangle as an example, Figure 1As shown, the weft yarns of the basic coating area 11 and the variable strength coating area 12 are arranged at the same interval, and any warp yarns in the basic area 121 of the variable strength coating area 12 are extended to the basic coating area 11, and continue to be the warp yarns of the basic coating area 11 and interlaced with the weft yarns of the basic coating area 11 one above and one below; in the variable strength coating area 12, a stitching area 122 is provided between any adjacent basic areas 121, and the warp yarns of the stitching area 122 only extend to the junction of the basic coating area 11 and the variable strength coating area 12, and in the basic coating area 11, at the position corresponding to the warp yarns in the stitching area 122, no warp yarns are interlaced with the weft yarns, that is, The number of warp yarns in the basic coating area 11 is less than that in the variable strength coating area 12. Accordingly, the warp yarn spacing in the basic coating area 11 is greater than that in the variable strength coating area 12. Generally, the warp yarn spacing in the basic coating area 11 is half of the warp yarn spacing in the variable strength coating area 12. Figure 1 As shown, any warp yarn is arranged longitudinally, and any weft yarn is perpendicular to the warp yarn and arranged horizontally. Figure 1 This is only a schematic diagram. In order to clearly describe the weaving structure of the yarn, the yarn fineness and the spacing between the yarns are enlarged for illustration. It does not mean that the actual distance and gap between the yarns are the size shown in the figure. Accordingly, in order to clearly show the floating length line 123, Figure 1 The shape of the floating yarn 123 is filled in, and the color of the actual floating yarn 123 is consistent with that of other warp yarns and weft yarns.

[0047] The above-mentioned coating 1 for the stent graft can be woven as follows: in the variable strength coating area 12, half of all the warp yarns are interlaced one above and one below to form the basic area 121, and the remaining half of the warp yarns are evenly distributed between each adjacent warp yarn in the basic area 121, wherein the number of warp and weft interlacing times and the number of warp and weft yarns at each interlacing change, either a warp yarn floats over three weft yarns and then interlaced with a weft yarn once to form a floating long line 123, or a warp yarn floats over four weft yarns and then interlaced with a weft yarn once to form a floating long line 123. The number of floating long lines 123 floating over the weft yarns is not limited to the above-mentioned three and four cases, and can also be five, six or more, that is, there can be a variety of interlacing methods to form floating long lines 123 of different lengths, which can be adjusted according to actual needs. When the fabric of the basic coating area 11 is woven, the number of warp and weft yarns is the same as that of the variable strength coating area 12, but among all the warp yarns, half of the warp yarns are evenly selected at intervals and are not interwoven during the weaving process, and the remaining half of the warp yarns are interwoven with the weft yarns: each warp yarn and each weft yarn are interwoven with each other up and down, and each interweaving forms a tissue point (i.e., a cross-shaped interweaving point); the non-interwoven warp yarns float outside the surface of the basic coating area 11, and after the fabric is woven, they can be cut off by cutting, trimming or tearing (the cutting position is generally the junction of the basic coating area 11 and the variable strength coating area 12).

[0048] In actual applications, in the coating 1 used for the stent graft, the axial coverage length, spacing distribution form and setting quantity of the basic coating area 11 and the variable strength coating area 12 can be adjusted according to different needs. Since the basic coating area 11 and the variable strength coating area 12 are spaced and staggered in the axial direction of the coating, the formed stent graft 100 has different strength areas in the axial direction, thereby forming a variable strength coating stent with greater flexibility and practicality.

[0049] As can be seen from the above, in the coating 1 for the stent graft proposed in this embodiment, only part of the warp yarns penetrate the basic coating area 11 and the variable strength coating area 12 at the same time, and the remaining part of the warp yarns only penetrate the variable strength coating area 12, and are not interwoven with the weft yarns of the basic coating area 11. Based on this, the basic coating area 11 removes part of the warp yarns compared to the variable strength coating area 12, thereby reducing the thickness and strength, and conversely improving the thickness and strength of the variable strength coating area 12. This method is equivalent to increasing the coating strength by increasing the weaving density of the warp yarns in the variable strength coating area 12, such as the EPI of the variable strength coating area 12 is 60, and the EPI of the basic coating area 11 is 30.

[0050] The technical effect of the coating 1 for the coated stent proposed in this technical solution is described in detail below.

[0051] 1) The coating strength of the basic coating area 11 is relatively basic, while the variable-strength coating area 12 provides a suture area with guaranteed strength for the coating, so that the coating is not prone to large pinholes and holes during suturing, which can effectively avoid the occurrence of internal leakage. The longer floating line area is convenient for the threading of the suture needle, reducing the difficulty of suturing the variable-strength coating area 12. Moreover, the coating areas with different strengths can be formed in a fabric weaving process, and there is no need to sew them together later. The overall coating thickness is about 0.2~0.3mm, which can be compressed in a relatively thinner outer sheath. With a thinner outer sheath, it is convenient to implant the coated stent by intervention during surgery, which is simpler to operate and reduces harm to patients.

[0052] 2) The yarn weaving methods of the basic coating area 11 and the variable strength coating area 12 are flexible, and a variety of reinforced area weaving can be achieved. The number and position of the variable strength coating area 12 are selective, and can be set in the proximal and distal areas of the coated stent, or in the middle area of ​​the coated stent without a stent.

[0053] 3) The number and position of the variable strength coating area 12 are selective and can be woven according to clinical use requirements.

[0054] 4) After the membrane is implanted, if the patient needs a second operation, there is no need to cut or remove the membrane. The variable strength membrane area 12 of the membrane can be directly sutured with other products, which greatly reduces the operation time, has a high success rate, and is simple to operate.

[0055] 5) It is convenient for the second-stage operation. The variable-strength coated area 12 can be directly sutured with the host blood vessel. The suture strength is guaranteed, and the blood vessel is not prone to tearing and bleeding, which solves the problem of easy bleeding during sewing of existing intracavitary coated stents.

[0056] 6) The coating can achieve changes in thickness and diameter. The variable thickness thin coating area can be used to sew metal stents. The coated stent prepared with it can be compressed into a small-caliber delivery device (such as a delivery sheath), which is more conducive to intracavitary surgical delivery and reduces the diameter of the delivery device. The coated stent prepared with a variable diameter coating can fit the autologous blood vessel better.

[0057] Embodiment 2.

[0058] The present embodiment proposes a method for preparing the coating 1 for the coated stent in the first embodiment, that is, weaving the basic coating area 11 and the variable strength coating area 12 into one body, including: interlacing a part of the warp yarns of the variable strength coating area 12 with all the weft yarns up and down to form a basic area 121, and interlacing the remaining part of the warp yarns with a weft yarn up and down to form a suture area 122 after each multiple weft yarns are continuously floated, so that the warp yarn part with multiple weft yarns continuously floated forms a floating long line 123, which is convenient for suture needle threading; then, part of the warp yarns of the variable strength coating area 12 are used to interlace the weft yarns of the basic coating area 11 up and down, and the remaining part of the warp yarns of the variable strength coating area 12 are cut off at the boundary between the variable strength coating area 12 and the basic coating area 11, so that the total number of warp yarns in the basic coating area 11 is less than the total number of warp yarns in the variable strength coating area 12.

[0059] Specifically, the coating 1 for the stent graft can be woven according to the following preparation process: in the variable strength coating area 12, half of all the warp yarns are interlaced one above and one below to form the basic area 121, and the remaining half of the warp yarns are evenly distributed between each adjacent warp yarn in the basic area 121, wherein the number of warp and weft interlacing times and the number of warp and weft yarns at each interlacing change, that is, a warp yarn may float over three weft yarns and then interlace with a weft yarn once to form a floating long line 123, or a warp yarn may float over four weft yarns and then interlace with a weft yarn once to form a floating long line 123. The number of floating long lines 123 floating over the weft yarns is not limited to the above three and four cases, and can also be five, six or more, that is, there can be a variety of interlacing methods to form floating long lines 123 of different lengths, which are adjusted according to actual needs. When the fabric of the basic coating area 11 is woven, the number of warp and weft yarns is the same as that of the variable strength coating area 12, but among all the warp yarns, half of the warp yarns are evenly selected at intervals and are not interwoven during the weaving process to achieve yarn reduction, and the remaining half of the warp yarns are interwoven with the weft yarns: each warp yarn and each weft yarn are interwoven with each other up and down, and each interweaving forms a tissue point (i.e., a cross-shaped interweaving point); the non-interwoven warp yarns float outside the surface of the basic coating area 11, and can be cut after the fabric is woven (the cutting position is generally the junction of the basic coating area 11 and the variable strength coating area 12).

[0060] In practical applications, in the coating 1 used for the coated stent, the axial coverage length, spacing distribution form and setting number of the basic coating area 11 and the variable strength coating area 12 can be adjusted according to different needs.

[0061] Embodiment three.

[0062] like Figure 2 As shown, this embodiment proposes a stent graft 100, including a graft and a corrugated stent 2, the graft is formed by rolling the graft 1 for the graft stent of the first embodiment, and a plurality of circles of corrugated stents 2 are arranged at intervals along the axial direction of the graft outside the basic graft area 11 of the graft. The arrangement of the corrugated stent 2 is a conventional structure of the graft stent in the art, and the specific structure and working principle are not repeated here.

[0063] In this embodiment, at least one of the first position, the second position and the third position of the coating is provided with a variable strength coating area 12, wherein the first position is the proximal end of the coating, the second position is the distal end of the coating, and the third position is any position between the proximal end and the distal end of the coating, such as a position without a corrugated stent 2. Figure 2 As shown in FIG. 1 , both the proximal and distal ends of the coating are provided with a variable strength coating area 12, but there is no variable strength coating area 12 between the proximal and distal ends. A corrugated support 2 is provided on at least one of the variable strength coating areas 12 of the proximal and distal ends, as shown in FIG. Figure 2As shown, a structure in which a corrugated support 2 is provided on the variable strength coating area 12 of the proximal end and the distal end.

[0064] Generally speaking, it is preferred that the corrugated stent 2 located in the variable strength coating area 12 has at least one of the values ​​of the stent wire diameter, the number of wave peaks and the amplitude not be greater than the corresponding values ​​of the corrugated stent 2 located in the basic coating area 11, and generally it is preferred to be less than that, which can reduce the pre-installed volume of the stent while ensuring the structural strength of the stent.

[0065] The technical effects of the coated stent 100 proposed in this technical solution are described in detail below.

[0066] 1) In the coating, the basic coating area 11 has a relatively basic coating strength, while the variable-strength coating area 12 provides a suture area with guaranteed strength for the coating, so that the coating is not prone to large pinholes and holes during suturing, which can effectively avoid the occurrence of internal leakage. The longer floating line area is convenient for the threading of the suture needle, reducing the difficulty of suturing the variable-strength coating area 12. Moreover, the coating areas with different strengths can be formed in a fabric weaving process, without the need to be sewn together later. The overall coating thickness is about 0.2~0.3mm, which can be compressed in a relatively thinner outer sheath. With a thinner outer sheath, it is convenient to implant the coated stent by intervention during surgery, which is simpler to operate and reduces harm to patients.

[0067] 2) The stent graft has a variable strength graft area 12 at the proximal and distal ends. When the surgeon needs to sew the stent graft to the artificial blood vessel during surgery, the longer floating thread in the variable strength graft area 12 facilitates the insertion of the suture needle. After suturing, large pinholes and holes are less likely to appear in the graft, which can effectively avoid the occurrence of internal leakage.

[0068] 3) After the stent graft is implanted, if the patient needs a second operation, there is no need to cut or remove the stent graft. The variable strength coated area 12 of the stent graft can be directly sutured with other products, which greatly reduces the operation time, has a high success rate, and is simple to operate.

[0069] 4) It is convenient for the second-stage operation. The variable-strength coated area 12 can be directly sutured with the host blood vessel, so the suture strength is guaranteed and the blood vessel is not prone to tearing and bleeding, thus solving the problem of easy bleeding during sewing of the existing intracavitary coated stent.

[0070] 5) The coating can achieve changes in thickness and diameter. The variable thickness thin coating area can be used to sew metal stents. The coated stent prepared with it can be compressed into a small-caliber delivery device (such as a delivery sheath), which is more conducive to intracavitary surgical delivery and reduces the diameter of the delivery device. The coated stent prepared with a variable diameter coating can fit the autologous blood vessel better.

[0071] 6) The proximal and distal ends of the stent graft have a variable strength graft area 12, which can reduce new hair dissection caused by the stent.

[0072] 7) The proximal and distal ends of the stent graft have a variable strength graft area 12, which is beneficial to the climbing of tissue and endothelium and better healing.

[0073] 8) The stent graft has a variable strength coated area 12 at the proximal and distal ends, which can reduce the incidence of type I endoleak by about 50%.

[0074] Embodiment 4.

[0075] like Figure 3 As shown, this embodiment proposes a stent graft 100, which differs from the third embodiment only in that the coating of the stent graft 100 of this embodiment is composed of a basic coating area 11 and three variable strength coating areas 12, and a variable strength coating area 12 is provided at the proximal and distal ends of the coating, respectively, and a corrugated stent 2 with a thinner wire diameter is sewn thereon. The variable strength coating area 12 at the proximal end can be sutured with an artificial blood vessel, and the variable strength coating area 12 at the distal end is convenient for in-situ sewing during surgery or secondary surgery. The remaining variable strength coating area 12 is located between the proximal and distal ends of the coating, and is arranged close to the distal end, so that the operator can cut the variable strength coating area 12 at the distal end of the stent graft according to actual needs and then suture the variable strength coating area 12.

[0076] The beneficial technical effects of the above-mentioned coated stent 100 can be found in Example 3, which will not be described in detail here.

[0077] Embodiment five.

[0078] like Figure 4 As shown, this embodiment proposes a stent graft 100, which is different from the fourth embodiment only in that no corrugated stent 2 is provided in any variable strength grafting area 12, and the rest is the same as the fourth embodiment and will not be described again.

[0079] Embodiment six.

[0080] like Figure 5 As shown, this embodiment provides a stent graft 100, which is composed of a basic graft region 11 and more than three variable strength graft regions 12, wherein a variable strength graft region 12 is provided at the proximal end and the distal end of the graft respectively, and other variable strength graft regions 12 are arranged at intervals between the proximal end and the distal end of the graft, such as Figure 5 As shown, a variable strength coating area 12 is provided between any two corrugated stents 2 between the proximal and distal ends of the coating. Among all the variable strength coating areas 12, some of the variable strength coating areas 12 are not provided with corrugated stents 2, and the remaining variable strength coating areas 12 are provided with corrugated stents 2. The variable strength coating area 12 at the proximal end can be sutured with the artificial blood vessel, the variable strength coating area 12 at the distal end is convenient for in-situ sewing during surgery or secondary surgery, and the variable strength coating areas 12 at the remaining positions can be used as suture areas for suture after the surgeon cuts the ends of the coated stent according to actual needs.

[0081] The technical effects of the coated stent 100 proposed in this technical solution are described in detail below.

[0082] 1) In the coating, the basic coating area 11 has a relatively basic coating strength, while the variable-strength coating area 12 provides a suture area with guaranteed strength for the coating, so that the coating is not prone to large pinholes and holes during suturing, which can effectively avoid the occurrence of internal leakage. The longer floating line area is convenient for the threading of the suture needle, reducing the difficulty of suturing the variable-strength coating area 12. Moreover, the coating areas with different strengths can be formed in a fabric weaving process, without the need to be sewn together later. The overall coating thickness is about 0.2~0.3mm, which can be compressed in a relatively thinner outer sheath. With a thinner outer sheath, it is convenient to implant the coated stent by intervention during surgery, which is simpler to operate and reduces harm to patients.

[0083] 2) The stent graft has a variable strength graft area 12 at the proximal and distal ends. When the surgeon needs to sew the stent graft to the artificial blood vessel during surgery, the longer floating thread in the variable strength graft area 12 facilitates the insertion of the suture needle. After suturing, large pinholes and holes are less likely to appear in the graft, which can effectively avoid the occurrence of internal leakage.

[0084] 3) After the stent graft is implanted, if the patient needs a second operation, there is no need to cut or remove the stent graft. The variable strength coated area 12 of the stent graft can be directly sutured with other products, which greatly reduces the operation time, has a high success rate, and is simple to operate.

[0085] 4) It is convenient for the second-stage operation. The variable-strength coated area 12 can be directly sutured with the host blood vessel, so the suture strength is guaranteed and the blood vessel is not prone to tearing and bleeding, thus solving the problem of easy bleeding during sewing of the existing intracavitary coated stent.

[0086] 5) The coating can achieve changes in thickness and diameter. The variable thickness thin coating area can be used to sew metal stents. The coated stent prepared with it can be compressed into a small-caliber delivery device (such as a delivery sheath), which is more conducive to intracavitary surgical delivery and reduces the diameter of the delivery device. The coated stent prepared with a variable diameter coating can fit the autologous blood vessel better.

[0087] 6) The proximal and distal ends of the stent graft have a variable strength graft area 12, which can reduce new hair dissection caused by the stent.

[0088] 7) The proximal and distal ends of the stent graft have a variable strength graft area 12, which is beneficial to the climbing of tissue and endothelium and better healing.

[0089] 8) The stent graft has a variable strength coated area 12 at the proximal and distal ends, which can reduce the incidence of type I endoleak by about 50%.

[0090] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A coating for a coated stent, characterized in that: The invention comprises a basic coating area and a variable-strength coating area arranged at intervals along the axial direction of the coating, wherein the basic coating area and the variable-strength coating area are both formed by interlacing warp yarns and weft yarns up and down, and the basic coating area and the variable-strength coating area are woven as a whole; wherein the total number of warp yarns in the variable-strength coating area is more than the total number of warp yarns in the basic coating area, or the total number of weft yarns in the variable-strength coating area is more than the total number of weft yarns in the basic coating area, or the total number of warp yarns in the variable-strength coating area is more than the total number of warp yarns in the basic coating area, and the total number of weft yarns in the variable-strength coating area is more than the total number of weft yarns in the basic coating area; wherein the warp yarns and weft yarns in the basic coating area are interlaced up and down, and the interlacing points of any warp yarn and any weft yarn form cross interlacing points; a part of the warp yarns in the variable-strength coating area are interlaced with all the weft yarns up and down to form the basic area, and the remaining part of the warp yarns are interlaced with one after floating multiple weft yarns in succession The weft yarns are interwoven up and down to form a stitching area, and the warp yarn parts of multiple weft yarns floated continuously form floating lines, the warp yarns in the stitching area are alternately arranged with the warp yarns in the basic area, and the intersection of any warp yarn and any weft yarn in the variable-strength coating area forms a cross-interweaving point; the weft yarns in the basic coating area and the variable-strength coating area are arranged at the same interval, and any warp yarn in the variable-strength coating area located in the basic area extends to the basic coating area, and the warp yarns of the basic coating area are interwoven with the weft yarns of the basic coating area up and down; in the variable-strength coating area, the stitching area is provided between any adjacent basic areas, and the warp yarns in the stitching area only extend to the junction of the basic coating area and the variable-strength coating area, and are cut off at the junction of the variable-strength coating area and the basic coating area, so that in the basic coating area, at the position corresponding to the warp yarn in the stitching area, no warp yarn is interwoven with the weft yarn.

2. The coating for stent graft according to claim 1, characterized in that: Any warp yarn and any weft yarn are polyester multifilaments with a fiber fineness of 20D-100D; or, any warp yarn and any weft yarn are polyester monofilaments; or, all warp yarns are polyester monofilaments and all weft yarns are polyester multifilaments; or, all warp yarns are polyester multifilaments and all weft yarns are polyester monofilaments.

3. The coating for stent graft according to claim 1, characterized in that: The coating is cylindrical or truncated cone-shaped.

4. The coating for stent graft according to claim 1, characterized in that: Any of the floating long lines continuously floats over more than three weft yarns.

5. A method for preparing a stent graft according to any one of claims 1 to 4, characterized in that: The basic coating area and the variable strength coating area are woven as a whole, including: a part of the warp yarns of the variable strength coating area are interlaced with all the weft yarns up and down to form a basic area, and the remaining part of the warp yarns are interlaced with a weft yarn up and down to form a stitching area after multiple weft yarns are continuously floated, so that the warp yarn part that continuously floats multiple weft yarns forms a floating long line; part of the warp yarns of the variable strength coating area are used to interlace with the weft yarns of the basic coating area up and down, and the remaining part of the warp yarns of the variable strength coating area are cut off at the boundary between the variable strength coating area and the basic coating area, so that in the basic coating area, at the position corresponding to the warp yarn in the stitching area, no warp yarn is interlaced with the weft yarn.

6. A stent graft, comprising a corrugated stent and a coating for a stent graft as claimed in any one of claims 1 to 4, wherein a plurality of circles of the corrugated stent are arranged at intervals along the axial direction of the coating outside the basic coating area of ​​the coating.

7. The stent graft according to claim 6, characterized in that: The variable strength coating area is provided at least at one of the first position, the second position and the third position of the coating, wherein the first position is the proximal end of the coating, the second position is the distal end of the coating, and the third position is any position between the proximal end and the distal end of the coating.

8. The stent graft according to claim 7, characterized in that: The corrugated bracket is arranged outside the variable strength coating area located at the first position and / or the second position, and the corrugated bracket located at the variable strength coating area is not greater than the corresponding value of the corrugated bracket located at the basic coating area in at least one of the bracket wire diameter, the number of wave peaks and the amplitude.