A comprehensive recovery method for black powder from waste ternary lithium batteries

Through the method of mixing concentrated sulfuric acid with water and mixing slurry and multi-step pH adjustment, the safety hazards and environmental pollution of medium and high temperature and high pressure recycling of ternary lithium battery black powder are solved, and efficient separation of nickel, cobalt, manganese and other elements is achieved. Recycling reduces production costs and environmental impacts.

CN118026280BActive Publication Date: 2024-11-19LEIYANG YANXIN NON FERROUS METALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410002910.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-02
Publication Date
2024-11-19
Estimated Expiration
2044-01-02

AI Technical Summary

Technical Problem

The existing ternary lithium battery black powder recycling methods have problems such as safety hazards, environmental pollution and low cobalt and nickel recovery rates, and are difficult to treat wastewater in the future.

Method used

After mixing concentrated sulfuric acid with water and mixing slurry, hydrogen peroxide and sulfite are added. Through the multi-step pH adjustment and precipitation process, the separation and enrichment of nickel, cobalt, manganese and other elements are achieved, and high temperature and high pressure conditions are avoided, and the process is simplified. Reduce wastewater pollution.

Benefits of technology

It has achieved efficient recycling of valuable elements such as nickel, cobalt, and manganese, reduced equipment investment and safety hazards, reduced environmental pollution, and has a high recovery rate and low production costs, which is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118026280B_ABST
    Figure CN118026280B_ABST
Patent Text Reader

Abstract

The invention relates to a comprehensive recovery method of waste ternary lithium battery black powder. The waste ternary lithium battery black powder is slurried and mixed with concentrated sulfuric acid to obtain a mixed slurry; the mixed slurry is reacted with hydrogen peroxide, and then water and sulfite are added. After the reaction, solid-liquid separation is performed to obtain a first clear liquid and a filter residue; alkali is added to the first clear liquid, and after the pH value is increased to 4.9-5.1, aging is performed, and solid-liquid separation is performed to obtain a second clear liquid and a copper-containing filter residue; alkali is added to the second clear liquid, and after the pH value is increased to 7-7.1, aging is performed, and solid-liquid separation is performed to obtain a third clear liquid and cobalt slag; after the third clear liquid is uniformly mixed with ethanolamine, sodium oxalate is added, and after no precipitation is generated, solid-liquid separation is performed to obtain a fourth clear liquid and nickel slag; alkali is added to the fourth clear liquid, and after the pH value is increased to 10-10.8, aging is performed, and solid-liquid separation is performed to obtain manganese slag and a fifth clear liquid rich in lithium. The invention can completely separate and recycle valuable elements such as Co, Ni, Li, Cu, Mn and the like in the black powder of waste ternary lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a comprehensive recovery method for waste ternary lithium battery black powder, belonging to the field of resource recovery and treatment of solid waste. Background Art

[0002] Due to its special advantages, ternary lithium batteries have been widely used in recent decades. Due to their limited repeated service life, a large number of batteries are scrapped every year. Because they contain valuable lithium, nickel, cobalt, and manganese, the scrapped batteries are recycled for comprehensive recycling, and lithium, nickel, cobalt, and manganese are separated, enriched, and impurities are removed to produce various products that can meet secondary use. In the past, several process methods have been developed to comprehensively recover lithium, nickel, and cobalt from waste ternary lithium battery black powder, such as: ① sulfuric acid roasting leaching separation method, ② high-pressure oxygen leaching separation method, and ③ atmospheric pressure sulfuric acid leaching mixed precipitation of cobalt, nickel, and ammonium persulfate separation method. These methods have their own applicability in actual use, but there are also some problems. First, the sulfuric acid roasting leaching separation method requires high-temperature sulfuric acid roasting, which causes serious environmental pollution. In particular, a small amount of plastic resin produces dioxin carcinogens when roasted at high temperature, which is very harmful and difficult to promote and adopt; second, the high-pressure oxygen leaching method requires a high temperature of about 250°C and a high pressure of about 30 MPa for the leaching process of this method, and the equipment investment cost is large, and its safety hazard is very large; third, the atmospheric pressure sulfuric acid leaching co-precipitation cobalt nickel ammonium persulfate separation method, the cobalt nickel leaching recovery rate is generally less than 95%, and the cobalt nickel co-precipitation needs to be subjected to subsequent re-dissolution and separation steps, and the process is long. More specifically, manganese is oxidized into manganese oxide with ammonium persulfate, and after filtering and solid-liquid separation, the mother liquor wastewater contains mixed soluble sulfates such as sodium sulfate and ammonium sulfate, which makes it difficult to deal with the wastewater in an environmentally friendly manner. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a comprehensive recovery method for waste ternary lithium battery black powder with simpler procedures, so as to achieve the recovery of valuable elements such as nickel, cobalt and manganese.

[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0005] A comprehensive recovery method for waste ternary lithium battery black powder comprises the following steps:

[0006] S1. Mix the waste ternary lithium battery black powder to be treated with water and prepare a slurry, then mix it with concentrated sulfuric acid and stir for 20-60 minutes to obtain a mixed slurry;

[0007] Among them, the ratio of waste ternary lithium battery black powder, water, and concentrated sulfuric acid is 1g: 1-2g: 1-1.5mL, preferably 1g: 1.2-1.8g: 1.1-1.4mL. The concentration of the concentrated sulfuric acid is ≥ 70wt%, preferably 90-99wt%, and more preferably 95-98wt%;

[0008] S2, mixing the mixed slurry with hydrogen peroxide, reacting for 10-90 minutes, then adding water and water-soluble sulfite, stirring at 50-70° C. for 20-60 minutes, and separating the solid and liquid to obtain a first clear liquid and a filter residue;

[0009] Among them, the amount of hydrogen peroxide added is 10-30wt% of the waste ternary lithium battery black powder corresponding to the mixed slurry, preferably 15-25wt%, the concentration of hydrogen peroxide is 20-40wt%, preferably 25-35wt%, the amount of water-soluble sulfite added is 6-25wt% of the waste ternary lithium battery black powder corresponding to the mixed slurry, preferably 10-20wt%; the amount of water added is 2-6 times the mass of the waste ternary lithium battery black powder corresponding to the mixed slurry, preferably 3-5 times;

[0010] S3, adding alkali or alkaline solution to the first clear liquid, and after the pH value of the reaction system is raised to 4.9-5.1, aging, solid-liquid separation, and obtaining a second clear liquid and a copper-containing filter residue; in this way, Fe in the first clear liquid can be reduced to 3+ 、Al 3+ , Cu 2+ The plasma is hydrolyzed to generate hydroxide precipitates that enter the copper-containing filter residue to achieve separation; preferably, the aging time is 10-120 minutes, more preferably 45-75 minutes; preferably, alkali or alkaline solution is added to the first clear liquid while stirring;

[0011] S4, adding alkali or alkali solution to the second clear liquid, and after the pH value of the reaction system is raised to 7-7.1, aging, solid-liquid separation, to obtain a third clear liquid and cobalt slag; preferably, the aging time is 10-120 min, more preferably 45-75 min; preferably, adding alkali or alkali solution to the second clear liquid while stirring;

[0012] S5, after the third clear liquid and ethanolamine are uniformly mixed, a water-soluble oxalate or a solution thereof is added until no precipitation is generated, and the solid-liquid separation is performed to obtain a fourth clear liquid and nickel slag;

[0013] During the addition of the water-soluble oxalate or its solution, the pH value of the reaction system is controlled to be 7-7.5 to prevent the manganese in the solution from being hydrolyzed and precipitated; the amount of ethanolamine added is 2-12wt% of the mass of the waste ternary lithium battery black powder corresponding to the third clear liquid, preferably 4-10wt%; preferably, the water-soluble oxalate or its solution is added while stirring;

[0014] S6, adding alkali or alkaline solution to the fourth clear solution, and after the pH value of the reaction system is increased to 10-10.8, aging, solid-liquid separation, and obtaining manganese slag and a fifth clear solution rich in lithium; preferably, the aging time is 10-120 minutes, more preferably 45-75 minutes. Preferably, the alkali or alkaline solution is added to the fourth clear solution while stirring.

[0015] The present invention first leaches and oxidizes under concentrated sulfuric acid conditions, so that each valuable element can be leached, and elements such as nickel, copper, cobalt, and aluminum can be oxidized; then reduction leaching is performed under dilute acid conditions to reduce cobalt to +2 valence. Subsequently, the pH value of the mixed slurry is adjusted so that elements such as copper, aluminum, and iron are first precipitated and separated, and the pH value is further adjusted so that Co is precipitated and separated in the form of Co(OH)2; then, ethanolamine and water-soluble oxalate are added so that nickel can be smoothly precipitated and separated in the form of nickel oxalate, and the pH value is further adjusted so that manganese is precipitated and separated in the form of manganese hydroxide, and a fifth clear liquid rich in lithium and alkaline is obtained. In this way, the separation and enrichment of valuable elements such as cobalt, nickel, manganese, and lithium can be achieved through one process, the process is simple and efficient, and the reaction conditions are mild, without the need for high temperature and high pressure equipment. Subsequently, there is no need to adjust the pH value of the fifth clear liquid, and lithium precipitation treatment can be directly performed, which helps to further simplify the process and save reagent consumption.

[0016] Furthermore, in the waste ternary lithium battery black powder to be treated, the Co content is 5-18wt%, the Ni content is 5-15wt%, the Li content is 1-8wt%, the Mn content is 3-10wt%, and preferably, the Cu content is 2-6wt%. Optionally, black powders with different components can be mixed in a certain ratio to obtain waste ternary lithium battery black powder that meets the above formula, so that each element can be balanced and stable for a long time, and after subsequent acid leaching with a fixed liquid-solid ratio, the content of each target element can be controlled under the concentration condition of 0.3-0.5mol / L, which provides a basis for the upper limit of element concentration for subsequent pH adjustment hydrolysis precipitation.

[0017] Further, in S1, concentrated sulfuric acid is slowly added into the reaction system.

[0018] Furthermore, in S2, the water-soluble sulfite includes one or more of sodium sulfite, potassium sulfite, and ammonium sulfite.

[0019] Generally, in S2, in the filter residue, Co≤1.0wt%, Ni≤0.8wt%, Li≤0.5wt%, Cu≤0.5%, Mn≤2wt%, and further, in the filter residue, Co≤0.2wt%, Ni≤0.1wt%, Li≤0.1wt%, Cu≤0.1%, Mn≤1wt%.

[0020] Generally, in S2, in the first clear liquid, the content of Co is 10-30 g / L, the content of Ni is 5-25 g / L, the content of Li is 5-15 g / L, the content of Cu is 2-8 g / L, and the content of Mn is 8-25 g / L.

[0021] Furthermore, in S3, in the second clear liquid, Fe≤0.002wt%, Al≤0.003wt%, Cu≤0.05wt%; further, in the copper-containing filter residue, the Cu content is 5-10wt%, and the precipitation separation rate of copper in the first clear liquid reaches more than 90-95%.

[0022] Further, in S3, S4 and S6, the alkali includes one or more of sodium hydroxide, potassium hydroxide and ammonia water, preferably sodium hydroxide. Preferably, in S3, S4 and S6, the alkali solution used is 1-3 mol / L sodium hydroxide solution.

[0023] Furthermore, in S4, the Co content in the third clear liquid is ≤0.001 g / L.

[0024] Optionally, the cobalt slag is washed with water, and then the solid and liquid are separated to obtain a cobalt hydroxide product with an iron, copper and aluminum content of less than 0.003wt%, which can be directly sold. Optionally, hot water is used for washing at a liquid-to-solid mass ratio of 2-6:1, and preferably, the temperature of the hot water is 50-60°C.

[0025] Furthermore, in S5, the water-soluble oxalate includes one or more of sodium oxalate, potassium oxalate, and ammonium oxalate.

[0026] Furthermore, in S5, the third clear liquid is mixed with ethanolamine, stirred for 20-40 minutes, and then a water-soluble oxalate or a solution thereof is added while stirring until no precipitation is generated, and then the solid and liquid are separated to obtain a fourth clear liquid and nickel slag.

[0027] Furthermore, in S5, the water-soluble oxalate solution is a saturated sodium oxalate solution.

[0028] Further, in S5, after no precipitation is generated and the Ni content in the reaction liquid is ≤0.002 g / L, solid-liquid separation is performed.

[0029] Furthermore, the nickel slag is washed with water, solid-liquid separated, and dried to obtain a nickel oxalate product with an impurity content of less than 0.003wt%, which can be directly sold. Optionally, hot water is used for washing at a liquid-solid mass ratio of 2-6:1, preferably, the temperature of the hot water is 50-60°C.

[0030] Furthermore, S6 is performed at room temperature.

[0031] Furthermore, after washing the manganese slag, the solid and liquid are separated and dried to obtain a manganese hydroxide product, which can be directly sold. Optionally, hot water is used for washing at a liquid-solid mass ratio of 2-6:1, and preferably, the temperature of the hot water is 50-60°C.

[0032] Furthermore, after S6, the fifth clear liquid is mixed with a water-soluble carbonate, and after lithium precipitation, the solid and liquid are separated to obtain a lithium carbonate product and a mother liquor. Preferably, during the lithium precipitation process, the temperature is controlled to be 80-95°C; preferably, stirring is performed during the lithium precipitation process. Preferably, the water-soluble carbonate is added until the lithium is completely reacted and precipitated, and the clear liquid is extracted later to observe whether there is any white precipitate of lithium carbonate produced, and if there is no white precipitate of lithium carbonate produced, the addition of the water-soluble carbonate can be stopped.

[0033] Optionally, after solid-liquid separation, the solid phase is washed with hot water at a liquid-solid mass ratio of 2-6:1, and dried to obtain a lithium carbonate product; preferably, the temperature of the hot water is 50-60° C. Generally, the content of Li2CO3 in the lithium carbonate product is ≥99%, and the impurities Fe, Al, Cu, Ni, Co, and Mn are all less than 0.003%, and it can be sold as electronic grade lithium carbonate.

[0034] Furthermore, the water-soluble carbonate includes one or more of sodium carbonate, potassium carbonate and ammonium carbonate.

[0035] Furthermore, after evaporating and crystallizing the mother liquor, solid-liquid separation (preferably centrifugal separation) is performed to obtain a sodium sulfate product and a residual liquid. The sodium sulfate product can be directly sold.

[0036] Furthermore, the remaining liquid is returned to the lithium precipitation step for recycling.

[0037] Furthermore, the water vapor generated by the evaporation is condensed to obtain condensed water, which is then returned to S1; preferably, the evaporation is a multiple-effect evaporation.

[0038] The comprehensive recovery method of the present invention can prevent serious flue gas pollution, reduce equipment investment and reduce production safety hazards, can safely and environmentally dispose of mother liquor wastewater, achieve zero pollution emissions, and has a high recovery rate of various metal elements and a low production cost.

[0039] The comprehensive recovery method of the present invention can fully separate and recover valuable elements such as Co, Ni, Li, Cu, Mn and the like in waste ternary lithium battery black powder. The recovery rate of elements such as Co, Ni, Li and the like can reach more than 95%, and the recovery rate of elements such as Cu and Mn and the like can reach more than 90%. The impurity content of the recovered products of each element is low, and all of them are high-purity and high-quality products with high product value. In addition, the production process is free of harmful gases and environmental pollution, and is carried out under normal pressure, thereby eliminating safety hazards such as high temperature and high pressure, and having low investment and production cost. The method can be widely promoted and applied, has huge environmental protection and social effects, high resource recovery benefits and excellent economic benefits, and has good prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The present invention is a flow chart of a comprehensive treatment method for waste ternary lithium battery black powder. DETAILED DESCRIPTION

[0041] The present invention will be described in detail below in conjunction with the embodiments. It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other. Unless otherwise specified, the relevant percentages refer to mass percentages.

[0042] Example 1

[0043] The processing process of the waste ternary lithium battery black powder in this embodiment is as follows:

[0044] Step 1: Take 1 kg of sample from 15t of waste ternary lithium battery raw materials, dry it at 104℃ for 4 hours, and randomly reserve 100g of waste ternary lithium battery black powder for testing; among them, the Ni content of the waste ternary lithium battery black powder is 9.6%, the Co content is 11.5%, the Li content is 2.9%, the Cu content is 3.9%, the Mn content is 5.6%, and the rest is organic matter such as graphite and plastic resin.

[0045] Step 2: add 200ml of water to a 1000ml beaker, slowly add 100ml of 98% concentrated sulfuric acid, add 100g of the waste ternary lithium battery black powder while stirring on a heating magnetic stirrer, and under this high sulfuric acid concentration condition, stir and leach for 30 minutes, then slowly add 50ml of hydrogen peroxide (concentration of 30%) to the solution in portions to prevent bubbles from bubbling, stir for 60 minutes, add 300ml of water to the beaker, continue stirring for 30 minutes, add 20g of Na2SO3 to the leachate, maintain the temperature at 60°C, and continue stirring for 60 minutes to complete the concentrated sulfuric acid oxidation leaching and dilute sulfuric acid reduction leaching process to obtain a leached slurry. This leaching stage can convert Ni, Co, Li, Cu, and Mn in the black powder into soluble sulfates.

[0046] Step 3: vacuum filter the leached slurry from step 2 to obtain 600 ml of filtered clear liquid and 47 g of leached residue (dry weight);

[0047] Among them, in the filtered clear liquid, the Ni content is 15.68g / L, the Co content is 18.59g / L, the Li content is 4.74g / L, the Cu content is 5.98g / L, and the Mn content is 8.4g / L. The leaching rates of each element are as follows: Ni 98%, Co 97%, Li 98%, Cu 92%, and Mn 90%.

[0048] Step 4: Pour the filtered clear liquid obtained in step 3 into a 1000 ml beaker, place it on a stirrer, adjust the magnetic stirring to high-speed strong stirring, slowly add 1 mol / L NaOH solution to the center of the vortex of the beaker with a pipette, adjust the pH of the leaching solution to slowly rise to pH 5.1 (taking about 20 minutes), and age it for 60 minutes to obtain slurry 1;

[0049] Among them, Fe in the solution during this process 3+ 、Al 3+ , Cu 2+ At pH 5.1, except for 0.02 g / L of Cu, the rest all form hydroxide precipitates.

[0050] Step 5: Filter the slurry 1 obtained in step 4 to obtain filter residue and clear liquid, wherein the filter residue can be sold as copper mud raw material, and the filtered clear liquid contains Fe≤0.001%, Al≤0.001%, and Cu≤0.02%.

[0051] Step 6: Slowly add 1 mol / L NaOH solution to the clear solution obtained in step 5 with a pipette, adjust the pH to 7.1 under high-speed strong stirring (about 15 minutes), and age for 60 minutes to hydrolyze the cobalt in the clear solution to form cobalt hydroxide, precipitate, and obtain slurry 2.

[0052] Step 7: filtering the slurry 2 of step 6 to obtain a cobalt hydroxide filter cake and a filtrate;

[0053] The cobalt hydroxide filter cake was stirred and washed with 300 ml of 60°C water, and then filtered to obtain the cobalt hydroxide product and the filtered clear liquid. The Co content in the clear liquid was ≤ 0.01 g / L.

[0054] The precipitation rate of cobalt in the clear solution obtained in step 5 is 99%.

[0055] Step 8: Add 8.7 g of ethanolamine (2-hydroxyethylamine) to the filtrate obtained in step 7, stir evenly, control the temperature of the reaction system to 60°C, and then add a saturated sodium oxalate solution thereto, still slowly adding while stirring, take three samples at a later stage, observe that no nickel precipitation is produced, stop adding, and obtain a nickel precipitate slurry;

[0056] During the reaction, the pH value of the reaction system was controlled at 7-7.5 using 1 mol / L NaOH solution.

[0057] Step nine: vacuum filter the nickel precipitate slurry in step eight to obtain a nickel oxalate filter cake and a filtered clear liquid, stir and wash the nickel oxalate filter cake with 300 ml of 60° C. water, filter, and dry to obtain 23.1 g of a nickel oxalate product;

[0058] Among them, Ni in the filtered clear liquid is ≤0.002%, and the nickel separation rate is 99%.

[0059] Step 10: Slowly add 1 mol / L NaOH solution to the filtered clear liquid obtained in step 9 with a pipette while stirring, so that the pH value of the reaction system is raised to 10.8, and age for 60 minutes. The manganese in the solution is precipitated to form manganese hydroxide to obtain manganese hydroxide slurry.

[0060] Step 11: vacuum filtration of the manganese hydroxide slurry obtained in step 10 to obtain a manganese hydroxide filter cake and a filtered clear liquid, which are washed with 300 ml of 60° C. water by stirring, filtered, and dried to produce a manganese hydroxide product;

[0061] Among them, Mn in the filtered clear liquid is ≤0.002%, and the separation rate of manganese is 99%.

[0062] Step 12: The filtered clear liquid obtained in step 11 is heated to 90° C., and a 3 mol / L Na2CO3 aqueous solution is added. When no white precipitate is produced after three visual inspections, the addition of Na2CO3 is stopped, and the reaction is stirred for about 60 minutes to produce lithium carbonate precipitate to obtain lithium carbonate slurry;

[0063] During this period, the main chemical reaction is: Li2SO4+Na2CO3=Li2CoO3↓+Na2SO4.

[0064] Step 13: Filter the lithium carbonate slurry obtained in step 12 to obtain a lithium carbonate filter cake and a filtered clear liquid, stir and wash the lithium carbonate filter cake with 300 ml of 60° C. water, and then filter to produce a Li2CO3 product;

[0065] Among them, Li in the filtered clear liquid is ≤0.002%, the lithium separation rate is 99%, and the remaining Na2SO4 is in the filtered clear liquid.

[0066] Step 14: Place the filtered clear liquid obtained in step 13 on an electric furnace for heating to evaporate and concentrate. In the later stage, due to the precipitation of Na2SO4 crystals, stir continuously to avoid boiling. When the volume of the solution in the beaker is concentrated to about 200 ml, stop heating and stirring to obtain a slurry.

[0067] Step 15: The concentrated slurry obtained in step 14 is vacuum filtered to obtain a sodium sulfate crystal cake and a mother liquor, and the mother liquor can be returned to step 14 for re-concentration.

[0068] After testing, the recovery rates of Co, Ni, Li, Cu and Mn were 96%, 97%, 97%, 91% and 89% respectively.

[0069] Comparative Example 1

[0070] Example 1 was repeated, except that the amount of Na2SO3 added in step 2 was 5 g.

[0071] The results show that the leached residue obtained in step 3 contains 4.65% Co.

[0072] Comparative Example 2

[0073] Example 1 was repeated, except that the amount of Na2SO3 added in step 2 was 0 g.

[0074] The results show that the leached residue obtained in step 3 contains 5.63% Co.

[0075] Comparative Example 3

[0076] Example 1 was repeated, except that the amount of ethanolamine added in step eight was 0.

[0077] The results showed that no obvious precipitate was produced in step eight and no nickel oxalate filter cake could be obtained.

[0078] Comparative Example 4

[0079] Example 1 was repeated, except that the amount of ethanolamine added in step eight was 1 g.

[0080] As a result, it was found that the amount of nickel oxalate product was 1.8 g.

[0081] Comparative Example 5

[0082] Example 1 was repeated, except that the pH value of the reaction system was not controlled in step eight.

[0083] The results showed that the manganese content in the nickel oxalate product reached 2.6%, indicating that manganese was also significantly precipitated in step eight.

[0084] The contents explained in the above embodiments should be understood as these embodiments are only used to more clearly illustrate the present invention, and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

Claims

1. A comprehensive recovery method for waste ternary lithium battery black powder, characterized in that: The method comprises the following steps: S1, mixing the waste ternary lithium battery black powder to be treated with water to prepare a slurry, mixing it with concentrated sulfuric acid, and stirring for 20-60 minutes to obtain a mixed slurry; The ratio of waste ternary lithium battery black powder, water and concentrated sulfuric acid is 1g:1-2g:1-1.5mL, and the concentration of the concentrated sulfuric acid is ≥70wt%; S2, mixing the mixed slurry with hydrogen peroxide, reacting for 10-90 minutes, then adding water and water-soluble sulfite, stirring at 50-70° C. for 20-60 minutes, and separating the solid and liquid to obtain a first clear liquid and a filter residue; The amount of hydrogen peroxide added is 10-30wt% of the waste ternary lithium battery black powder corresponding to the mixed slurry, the concentration of hydrogen peroxide is 20-40wt%, the amount of water-soluble sulfite added is 6-25wt% of the waste ternary lithium battery black powder corresponding to the mixed slurry; the amount of water added is 2-6 times the mass of the waste ternary lithium battery black powder corresponding to the mixed slurry; S3, adding alkali or alkaline solution to the first clear liquid, and after the pH value of the reaction system is raised to 4.9-5.1, aging, solid-liquid separation, and obtaining a second clear liquid and copper-containing filter residue; S4, adding alkali or alkaline solution to the second clear liquid, and after the pH value of the reaction system is raised to 7-7.1, aging, solid-liquid separation, and obtaining a third clear liquid and cobalt slag; S5, after the third clear liquid and ethanolamine are uniformly mixed, a water-soluble oxalate or a solution thereof is added until no precipitation is generated, and the solid-liquid separation is performed to obtain a fourth clear liquid and nickel slag; Wherein, during the addition of water-soluble oxalate or its solution, the pH value of the reaction system is controlled to be 7-7.5; the amount of ethanolamine added is 2-12wt% of the mass of the waste ternary lithium battery black powder corresponding to the third clear liquid; S6. Add alkali or alkali solution to the fourth clear liquid, and after the pH value of the reaction system increases to 10-10.8, age and separate the solid and liquid to obtain manganese slag and a fifth clear liquid rich in lithium.

2. The comprehensive recovery method according to claim 1, characterized in that: The waste ternary lithium battery black powder to be processed has a Co content of 5 to 18 wt %, a Ni content of 5 to 15 wt %, a Li content of 1 to 8 wt %, and a Mn content of 3 to 10 wt %.

3. The comprehensive recovery method according to claim 2, characterized in that: The Cu content in the waste ternary lithium battery black powder to be processed is 2-6wt%.

4. The comprehensive recovery method according to claim 1, characterized in that: In S2, the water-soluble sulfite includes one or more of sodium sulfite, potassium sulfite, and ammonium sulfite.

5. The comprehensive recovery method according to claim 1, characterized in that: In S3, S4 and S6, the alkali includes one or more of sodium hydroxide, potassium hydroxide and ammonia water.

6. The comprehensive recovery method according to claim 5, characterized in that: In S3, S4 and S6, the base is sodium hydroxide.

7. The comprehensive recovery method according to claim 1, characterized in that: In S5, the water-soluble oxalate includes one or more of sodium oxalate, potassium oxalate, and ammonium oxalate.

8. The comprehensive recovery method according to claim 1, characterized in that: After S6, the fifth clear liquid is mixed with a water-soluble carbonate, and after lithium precipitation, the solid and liquid are separated to obtain a lithium carbonate product and a mother liquor.

9. The comprehensive recovery method according to claim 8, characterized in that: The water-soluble carbonate includes one or more of sodium carbonate, potassium carbonate and ammonium carbonate.

10. The comprehensive recovery method according to claim 8, characterized in that: After evaporating and crystallizing the mother liquor, the solid and liquid are separated to obtain a sodium sulfate product and a residual liquid.

11. The comprehensive recovery method according to claim 10, characterized in that: The remaining solution is returned to the lithium precipitation step.

12. The comprehensive recovery method according to claim 10, characterized in that: The water vapor generated by evaporation is condensed to obtain condensed water, which is then returned to S1.

13. The comprehensive recovery method according to claim 12, characterized in that: The evaporation is a multiple-effect evaporation.

Citation Information

Patent Citations

  • Recycling method for valuable metal from waste nickel-cobalt-manganese lithium ion battery

    CN107653378A

  • Grading recovery method for waste ternary lithium battery

    CN109182732A

  • Method for separating and recycling nickel, cobalt, manganese and lithium from waste ternary lithium battery

    CN114717419A

  • Method for recycling nickel, cobalt and manganese from waste ternary lithium battery through fractional precipitation

    CN115216620A

  • Method for recovering nickel, cobalt and manganese from waste ternary lithium battery

    CN116287718A