A gel-injected ceramic microbead and preparation method thereof

Ceramic microspheres were prepared by gel casting, and polyethylene glycol and γ-aminopropyltriethoxysilane were used to improve the dispersibility of the components. Nano-titanium dioxide and nano-silica were used to reinforce the fillers, which solved the problem of insufficient strength and wear resistance of ceramic balls and achieved ceramic microspheres with high wear resistance and high strength.

CN118026651BActive Publication Date: 2024-11-08SANZE SHANGHAI NEW MATERIAL TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410135318.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-31
Publication Date
2024-11-08
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Existing ceramic ball manufacturing processes cannot simultaneously achieve high bulk density, strength, hardness, and excellent stability, resulting in poor grinding efficiency and usage stability.

Method used

Ceramic microspheres with high uniformity and strength were prepared by using gel casting method, with polyethylene glycol and γ-aminopropyltriethoxysilane as solvents and modifiers, and nano-titanium dioxide and nano-silica as wear-resistant powders.

Benefits of technology

This improved the wear resistance and strength of ceramic microspheres, ensuring the stability and efficiency of the grinding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004691041870000071
    Figure BDA0004691041870000071
  • Figure BDA0004691041870000081
    Figure BDA0004691041870000081
Patent Text Reader

Abstract

The present application relates to the technical field of ceramic microspheres, and specifically discloses a gel-injected ceramic microsphere and a preparation method thereof. A gel-injected ceramic microsphere, the raw materials of which include the following components in parts by weight: 18 to 25 parts of water, 0.3 to 0.7 parts of polyethylene glycol, 2 to 5 parts of monomers, 0.2 to 0.3 parts of cross-linking agents, 0.2 to 0.5 parts of defoaming agents, 0.1 to 0.3 parts of dispersants, 0.1 to 0.5 parts of catalysts, 1 to 5 parts of initiators, 1 to 2.5 parts of sintering aids, and 90 to 110 parts of ceramic powder. In the present application, polyethylene glycol is added to the raw materials to alleviate the oxidation phenomenon of the slurry surface, so that the components in the raw materials are evenly dispersed, and ceramic microspheres with uniformity and high strength are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of ceramic microspheres, and in particular to a gel-injected ceramic microsphere and a preparation method thereof. Background Art

[0002] Grinding media balls, as a main grinding medium, are generally divided into two categories. Metal grinding media balls include high manganese steel balls, carbon steel balls, alloyed cast iron balls and various alloy iron balls. Non-metallic grinding media balls are further divided into organic polymer grinding balls and inorganic non-metallic grinding balls. Among them, polytetrafluoroethylene is the most commonly used organic polymer material. In addition to traditional natural ball stones such as agate, gravel, and pebbles, inorganic non-metallic materials also include oxide ceramic grinding balls such as alumina and zirconium oxide, carbide ceramic grinding balls such as silicon carbide and tungsten carbide, and composite ceramic grinding balls such as zirconium silicate and silicon nitride. Among them, oxide and non-oxide ceramic grinding media balls are relatively widely used.

[0003] Commonly used ceramic ball preparation processes include plastic extrusion molding, rolling molding, isostatic pressing, etc. The plastic extrusion molding method has a small investment and production scale, simple equipment, but the product has a low firing temperature, low density, and large wear, and has now been gradually eliminated by the market; the rolling molding method is a commonly used preparation method, and the output of the prepared grinding medium balls is large, but the requirements for raw materials are high, and there are certain operational difficulties, which easily makes the prepared beads have poor sphericity, many microscopic defects on the surface of the microspheres, and poor wear resistance, thereby affecting the grinding efficiency and stability of use; the products prepared by the isostatic pressing method have poor wear resistance, because the uneven moisture content of the powder and the inappropriate granulation size can easily cause the ball blank to crack during the molding process, and the wear resistance deteriorates. Although the above-mentioned ceramic ball preparation processes are relatively mature and can prepare ceramic medium balls for grinding, these ceramic medium balls all have certain defects and cannot simultaneously have the characteristics of high relative volume density, high strength and hardness, and excellent stability. Summary of the invention

[0004] In order to improve the strength of the prepared ceramic microspheres, the present application provides a gel-injected ceramic microsphere and a preparation method thereof.

[0005] In the first aspect, the present application provides a gel-injected ceramic microbead, which adopts the following technical solution:

[0006] The invention discloses a gel-injected ceramic microbead. The raw materials of the ceramic microbead include the following components in parts by weight: 18 to 25 parts of water, 0.3 to 0.7 parts of polyethylene glycol, 2 to 5 parts of monomers, 0.2 to 0.3 parts of cross-linking agent, 0.2 to 0.5 parts of defoaming agent, 0.1 to 0.3 parts of dispersant, 0.1 to 0.5 parts of catalyst, 1 to 5 parts of initiator, 1 to 2.5 parts of sintering aid and 90 to 110 parts of ceramic powder.

[0007] By adopting the above technical solution and adding polyethylene glycol to the raw materials, the phenomenon of surface oxidation of the slurry can be alleviated, so that the components in the raw materials are evenly dispersed, and ceramic microbeads with uniformity and high strength are obtained.

[0008] In a specific embodiment, the raw material of the ceramic microbeads further includes 0.1 to 0.3 parts by weight of a reinforcing filler, and the raw material of the reinforcing filler includes wear-resistant powder, γ-aminopropyltriethoxysilane, and ethanol.

[0009] By adopting the above technical scheme, ethanol is used as a solvent, so that γ-aminopropyltriethoxysilane can wrap the wear-resistant powder, thereby improving the dispersion performance of the wear-resistant powder. The wear-resistant powder is evenly dispersed in the ceramic microbeads, thereby improving the wear resistance of the ceramic microbeads. In addition, γ-aminopropyltriethoxysilane can further cross-link the components in the raw materials, thereby improving the strength of the ceramic microbeads.

[0010] In a specific embodiment, the method for preparing the reinforcing filler comprises the following steps:

[0011] Add γ-aminopropyltriethoxysilane and ethanol into water, stir and mix evenly to obtain a modified solution;

[0012] The wear-resistant powder is stirred and mixed evenly. During the stirring process, the modified liquid is sprayed into the wear-resistant powder. After the spraying is completed, the powder is stirred and dried to obtain a reinforced filler.

[0013] By adopting the above technical scheme, γ-aminopropyltriethoxysilane is first dissolved in ethanol to obtain a modified liquid, and then the modified liquid is sprayed on the wear-resistant powder and dried, and the γ-aminopropyltriethoxysilane is wrapped on the wear-resistant powder to obtain a reinforcing filler with good dispersibility.

[0014] In a specific embodiment, the weight ratio of the modified liquid to the wear-resistant powder is 1:(13-14).

[0015] By adopting the above technical solution, the ratio of the modified liquid to the wear-resistant powder is further limited, and the modification effect of γ-aminopropyltriethoxysilane on the wear-resistant powder is improved.

[0016] In a specific embodiment, the wear-resistant powder comprises a mixture of nano-titanium dioxide and nano-silicon dioxide, and the weight ratio of the nano-titanium dioxide to the nano-silicon dioxide is 1:(2-3).

[0017] By adopting the above technical solution, the wear-resistant powder is a mixture of nano titanium dioxide and nano silicon dioxide. Nano titanium dioxide and nano silicon dioxide have high hardness. The combination of the two improves the wear resistance of the ceramic micro beads.

[0018] In a specific embodiment, the monomer includes one of acrylamide and methacrylamide.

[0019] In a specific embodiment, the sintering aid includes a mixture of carbon black and boron carbide.

[0020] In a specific embodiment, the ceramic powder includes one or more of aluminum oxide, zirconium oxide, magnesium oxide, silicon carbide, and silicon nitride.

[0021] In a second aspect, the present application provides a method for preparing gel-injected ceramic microspheres, which adopts the following technical solution:

[0022] A method for preparing gel-injected ceramic microspheres comprises the following steps:

[0023] Preparation of gel grouting material: monomer, cross-linking agent, defoamer, dispersant, polyethylene glycol and deionized water are prepared into a premixed liquid, pH of the premixed liquid is adjusted to 10-11 with a pH adjuster, reinforcing filler, sintering aid and ceramic powder are continuously added under stirring of a stirrer, stirring speed is gradually increased as the amount of powder added, and stirring is carried out at a speed of 600-800 r / min to obtain gel grouting material;

[0024] Solidification and thickening of slurry: Add catalyst to gel grouting material at 15-20°C, add initiator to initiate slurry solidification after vacuum degassing, and the slurry gradually starts to thicken to obtain uncured slurry;

[0025] Preparation of microbeads: Place a thin plate coated with a release agent on the uncured slurry and apply downward pressure to form regular spherical microbeads. Then remove the pressure. After the slurry thickens, hold the thin plate to prevent displacement. After the slurry is completely cured, the gel-injected ceramic microbeads are lifted from the slurry together with the thin plate to obtain spherical microbeads. After sintering, ceramic microbeads are obtained.

[0026] By adopting the above technical scheme, the raw materials are first mixed evenly to obtain a gel grouting material, and then a catalyst and a curing agent are added to allow the gel grouting material to slowly solidify. At the same time, the slurry is squeezed downward with a thin plate with round holes to obtain spherical microbeads, and finally the spherical microbeads are sintered to obtain ceramic microbeads with higher strength.

[0027] In a specific possible implementation manner, the thin plate is provided with regular circular holes with a diameter of 0.1-0.3 mm, and the thickness of the thin plate is 0.5 mm.

[0028] In summary, the present application includes at least one of the following beneficial technical effects:

[0029] 1. In this application, polyethylene glycol is added to the raw materials to alleviate the phenomenon of surface oxidation of the slurry, so that the components in the raw materials are evenly dispersed, and ceramic microbeads with uniformity and high strength are obtained;

[0030] 2. In the present application, ethanol is used as a solvent, so that γ-aminopropyltriethoxysilane can encapsulate the wear-resistant powder, thereby improving the dispersibility of the wear-resistant powder. The wear-resistant powder is evenly dispersed in the ceramic microbeads, thereby improving the wear resistance of the ceramic microbeads. In addition, γ-aminopropyltriethoxysilane can further cross-link the components in the raw materials, thereby improving the strength of the ceramic microbeads.

[0031] 3. The method of the present application first mixes the raw materials evenly to obtain a gel grouting material, then adds a catalyst and a curing agent to allow the gel grouting material to slowly solidify. At the same time, a thin plate with a circular hole is used to extrude the slurry downward to obtain spherical microbeads, and finally the spherical microbeads are sintered to obtain ceramic microbeads with higher strength. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] All raw materials in the examples can be obtained commercially. The monomer includes but is not limited to one of acrylamide and methacrylamide, and in this application, it is acrylamide; the ceramic powder includes but is not limited to a mixture of one or more of aluminum oxide, zirconium oxide, magnesium oxide, silicon carbide, and silicon nitride, and in this application, it is zirconium oxide; and the defoamer is an OTD defoamer.

[0034] Preparation Example

[0035] Preparation Example 1

[0036] Preparation Example 1 provides a method for preparing a reinforcing filler, comprising the following steps:

[0037] Add γ-aminopropyltriethoxysilane and ethanol into water, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol and water is 5:18:2;

[0038] Add the wear-resistant powder into the mixer and mix evenly. During the stirring process, spray the modifying liquid into the wear-resistant powder. After the spraying is completed, continue stirring for 0.5 hours and dry at 110°C for 1 hour to obtain a reinforced filler; wherein the wear-resistant powder includes a mixture of nano-titanium dioxide and nano-silicon dioxide, and the weight ratio of nano-titanium dioxide to nano-silicon dioxide is 1:2.5; the weight ratio of the modifying liquid to the wear-resistant powder is 1:12.5.

[0039] Preparation Example 2

[0040] The difference between Preparation Example 2 and Preparation Example 1 is that the weight ratio of the modified liquid to the wear-resistant powder is 1:13; the remaining steps are consistent with Preparation Example 1.

[0041] Preparation Example 3

[0042] The difference between Preparation Example 3 and Preparation Example 1 is that the weight ratio of the modified liquid to the wear-resistant powder is 1:13.5; the remaining steps are consistent with Preparation Example 1.

[0043] Preparation Example 4

[0044] The difference between Preparation Example 4 and Preparation Example 1 is that the weight ratio of the modified liquid to the wear-resistant powder is 1:14; the remaining steps are consistent with Preparation Example 1.

[0045] Preparation Example 5

[0046] The difference between Preparation Example 5 and Preparation Example 1 is that the weight ratio of the modified liquid to the wear-resistant powder is 1:14.5; the remaining steps are consistent with Preparation Example 1.

[0047] Preparation Example 6

[0048] The difference between Preparation Example 6 and Preparation Example 3 is that the wear-resistant powder includes nano-titanium dioxide; the remaining steps are consistent with Preparation Example 3.

[0049] Preparation Example 7

[0050] The difference between Preparation Example 7 and Preparation Example 3 is that the wear-resistant powder includes nano-silicon dioxide; the remaining steps are consistent with Preparation Example 3.

[0051] Example

[0052] Example 1

[0053] Embodiment 1 provides a method for preparing gel-injected ceramic microspheres, comprising the following steps:

[0054] Preparation of gel grouting material: 2kg monomer, 0.2kg cross-linking agent, 0.2kg defoaming agent, 0.1kg dispersant, 0.3kg polyethylene glycol and 18kg deionized water are stirred and mixed evenly to prepare a premixed liquid, and the pH of the premixed liquid is adjusted to 10-11 with a pH regulator, and 1kg sintering aid and 90kg ceramic powder are continuously added under stirring of a stirrer, and the stirring speed is gradually increased as the amount of powder added is increased, and the mixture is stirred at a speed of 700r / min to obtain a gel grouting material; wherein the monomer is acrylamide; the cross-linking agent is N,N-methylenebisacrylamide; the dispersant is citric acid; the sintering aid is a mixture of carbon black and boron carbide, and the weight ratio of carbon black to boron carbide is 2.5:1; the ceramic powder is zirconium oxide;

[0055] Solidification and thickening of the slurry: At 18°C, 0.1 kg of catalyst was added to the gel grouting material, and after vacuuming and defoaming, 1 kg of initiator was added to initiate the slurry solidification. The slurry gradually began to thicken to obtain uncured slurry; the catalyst was tetramethylethylenediamine; the initiator was ammonium persulfate;

[0056] Preparation of microbeads: a thin plate coated with a release agent is placed on the uncured slurry, and downward pressure is applied to form regular spherical microbeads, and then the pressure is released. After the slurry thickens, the thin plate is supported to prevent displacement. After the slurry is completely cured, the gel-injected ceramic microbeads are lifted from the slurry together with the thin plate to obtain spherical microbeads, which are sintered to obtain ceramic microbeads; wherein the thin plate is provided with a plurality of regular circular holes with a diameter of 0.1-0.3 mm, and the thickness of the thin plate is 0.5 mm.

[0057] Example 2

[0058] The difference between Example 2 and Example 1 is that, the gel grouting material is prepared: 3.5kg of monomer, 0.25kg of cross-linking agent, 0.35kg of defoaming agent, 0.2kg of dispersant, 0.5kg of polyethylene glycol and 22kg of deionized water are stirred and mixed evenly to form a premix, the pH of the premix is ​​adjusted to 10-11 with a pH regulator, 1.8kg of sintering aid and 100kg of ceramic powder are continuously added under stirring with a stirrer, the stirring speed is gradually increased as the amount of powder added, and the gel grouting material is obtained at a speed of 700r / min; solidification and thickening of the slurry: at 18°C, 0.3kg of catalyst is added to the gel grouting material, and after vacuuming and defoaming, 3kg of initiator is added to initiate the slurry solidification, the slurry gradually begins to thicken, and an uncured slurry is obtained; the remaining steps are consistent with Example 1.

[0059] Example 3

[0060] The difference between Example 3 and Example 1 is that the gel grouting material is prepared by stirring and mixing 5 kg of monomer, 0.3 kg of cross-linking agent, 0.5 kg of defoaming agent, 0.3 kg of dispersant, 0.7 kg of polyethylene glycol and 25 kg of deionized water to form a premix, adjusting the pH of the premix to 10-11 with a pH regulator, continuously adding 2.5 kg of sintering aid and 110 kg of ceramic powder under stirring with a stirrer, gradually increasing the stirring speed as the amount of powder added, and stirring at a speed of 700 r / min to obtain a gel grouting material;

[0061] Solidification and thickening of the slurry: At 18°C, 0.5 kg of catalyst was added to the gel grouting material. After vacuuming and degassing, 5 kg of initiator was added to initiate the slurry solidification. The slurry gradually began to thicken to obtain uncured slurry. The remaining steps were consistent with Example 1.

[0062] Example 4

[0063] The difference between Example 4 and Example 2 is that the sintering aid is carbon black; the remaining steps are consistent with Example 2.

[0064] Example 5

[0065] The difference between Example 5 and Example 2 is that the sintering aid is boron carbide; the remaining steps are consistent with Example 2.

[0066] Example 6

[0067] The difference between Example 6 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH regulator, and 0.2 kg of the reinforcing filler in Preparation Example 1, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added under stirring with a stirrer. The stirring speed is gradually increased with the addition amount of powder, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material; the remaining steps are consistent with Example 2.

[0068] Example 7

[0069] The difference between Example 7 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH regulator. Under stirring with a stirrer, 0.2 kg of the reinforcing filler in Preparation Example 2, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added. As the amount of powder added increases, the stirring speed is gradually increased, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material. The remaining steps are consistent with Example 2.

[0070] Example 8

[0071] The difference between Example 8 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH regulator, and 0.2 kg of the reinforcing filler in Preparation Example 3, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added under stirring with a stirrer. The stirring speed is gradually increased with the addition of powder, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material; the remaining steps are consistent with Example 2.

[0072] Example 9

[0073] The difference between Example 9 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH adjuster. Under stirring with a stirrer, 0.2 kg of the reinforcing filler in Preparation Example 4, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added. As the amount of powder added increases, the stirring speed is gradually increased, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material. The remaining steps are consistent with Example 2.

[0074] Example 10

[0075] The difference between Example 10 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH regulator. Under stirring in a stirrer, 0.2 kg of the reinforcing filler in Preparation Example 5, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added. As the amount of powder added increases, the stirring speed is gradually increased, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material. The remaining steps are consistent with Example 2.

[0076] Embodiment 11

[0077] The difference between Example 11 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH adjuster. Under stirring with a stirrer, 0.2 kg of the reinforcing filler in Preparation Example 6, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added. As the amount of powder added increases, the stirring speed is gradually increased, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material. The remaining steps are consistent with Example 2.

[0078] Example 12

[0079] The difference between Example 12 and Example 2 is that, in the step of preparing the gel grouting material, 3.5 kg of monomer, 0.25 kg of cross-linking agent, 0.35 kg of defoaming agent, 0.2 kg of dispersant, 0.5 kg of polyethylene glycol and 22 kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH adjuster. Under stirring with a stirrer, 0.2 kg of the reinforcing filler in Preparation Example 7, 1.8 kg of sintering aid and 100 kg of ceramic powder are continuously added. As the amount of powder added increases, the stirring speed is gradually increased, and the mixture is stirred at a speed of 700 r / min to obtain the gel grouting material. The remaining steps are consistent with Example 2.

[0080] Comparative Example

[0081] Comparative Example 1

[0082] The difference between Comparative Example 1 and Example 1 is that, in preparing the gel grouting material, 2kg of monomer, 0.2kg of cross-linking agent, 0.2kg of defoaming agent, 0.1kg of dispersant and 18.3kg of deionized water are stirred and mixed evenly to form a premix, and the pH of the premix is ​​adjusted to 10-11 with a pH adjuster. 1kg of sintering aid and 90kg of ceramic powder are continuously added under stirring in a stirrer. The stirring speed is gradually increased as the amount of powder added is increased, and the mixture is stirred at a speed of 700r / min to obtain the gel grouting material. The remaining steps are consistent with Example 1.

[0083] Performance testing

[0084] The ceramic microbeads in each embodiment and comparative example were sent to a testing device to obtain Mohs hardness and average wear.

[0085] Table 1 Performance test results of ceramic microspheres

[0086]

[0087]

[0088] Combining Example 1 and Comparative Example 1, the ceramic microbeads in Example 1 have higher hardness and better wear resistance. It can be seen that when preparing the gel grouting material, adding polyethylene glycol to the raw materials can alleviate the oxidation phenomenon of the slurry surface, so that the components in the raw materials are evenly dispersed, thereby improving the hardness and wear resistance of the prepared ceramic microbeads.

[0089] In combination with Examples 1-3, the wear resistance of the ceramic microbeads in Example 2 is the best. It can be seen that when preparing the ceramic microbeads, increasing the amount of raw materials used will result in the wear resistance of the ceramic microbeads showing a trend of first increasing and then decreasing.

[0090] Combining Example 2, Example 4 and Example 5, the wear resistance of the ceramic microbeads in Example 2 is the best. It can be seen that when preparing the gel grouting material, the sintering aid is preferably a mixture of carbon black and boron carbide, and the performance of the obtained ceramic microbeads is better.

[0091] Combining Example 2 and Example 6, the wear resistance of the ceramic microbeads in Example 6 is better. It can be seen that when preparing the gel grouting material, adding the wear-resistant powder modified by γ-aminopropyltriethoxysilane to the raw materials improves the wear resistance of the ceramic microbeads.

[0092] Combined with Examples 6-10, the wear resistance of the ceramic microbeads in Examples 7-9 is good. It can be seen that when preparing reinforcing fillers, the ratio of the modified liquid to the wear-resistant powder is preferably 1: (13-14), and the dispersion effect of the wear-resistant powder is better, thereby improving the wear resistance of the ceramic microbeads.

[0093] Combining Example 8, Example 11 and Example 12, the ceramic microbeads in Example 8 have the best wear resistance. It can be seen that when preparing reinforcing fillers, the wear-resistant powder is preferably a mixture of nano-titanium dioxide and nano-silicon dioxide, and the ceramic microbeads finally obtained have good wear resistance.

[0094] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for preparing gel-injected ceramic microspheres, characterized in that: The following steps are involved: Preparation of gel grouting material: monomer, cross-linking agent, defoamer, dispersant, polyethylene glycol and deionized water are prepared into a premixed liquid, pH of the premixed liquid is adjusted to 10-11 with a pH regulator, reinforcing filler, sintering aid and ceramic powder are continuously added under stirring of a stirrer, stirring speed is gradually increased as the amount of powder added, and stirring is carried out at a speed of 600-800r / min to obtain gel grouting material; Solidification and thickening of the slurry: at 15-20°C, a catalyst is added to the gel grouting material, and after vacuuming and defoaming, an initiator is added to initiate the solidification of the slurry, and the slurry gradually begins to thicken to obtain an uncured slurry; the raw materials of the ceramic microbeads include the following components in parts by weight: 18-25 parts of deionized water, 0.3-0.7 parts of polyethylene glycol, 2-5 parts of monomers, 0.2-0.3 parts of cross-linking agents, 0.2-0.5 parts of defoaming agents, 0.1-0.3 parts of dispersants, 0.1-0.5 parts of catalysts, 1-5 parts of initiators, 1-2.5 parts of sintering aids, 90-110 parts of ceramic powder, and 0.1-0.3 parts of reinforcing fillers; the sintering aids include a mixture of carbon black and boron carbide; the raw materials of the reinforcing fillers include wear-resistant powder, γ-aminopropyltriethoxysilane, and ethanol; the preparation method of the reinforcing fillers includes the following steps: Add γ-aminopropyltriethoxysilane and ethanol into water, stir and mix evenly to obtain a modified solution; The wear-resistant powder is stirred and mixed evenly, and during the stirring process, a modifying liquid is sprayed into the wear-resistant powder. After the spraying is completed, the modified liquid is continued to be stirred and dried to obtain a reinforced filler; the weight ratio of the modifying liquid to the wear-resistant powder is 1: (13-14); the wear-resistant powder includes a mixture of nano-titanium dioxide and nano-silicon dioxide, and the weight ratio of the nano-titanium dioxide to the nano-silicon dioxide is 1: (2-3); Preparation of microbeads: a thin plate coated with a release agent is placed on the uncured slurry, and downward pressure is applied to form regular spherical microbeads, and then the pressure is released. After the slurry thickens, the thin plate is supported to prevent displacement. After the slurry is completely cured, the gel-injected ceramic microbeads are lifted from the slurry together with the thin plate to obtain spherical microbeads, which are sintered to obtain ceramic microbeads. The thin plate is provided with regular circular holes with a diameter of 0.1-0.3 mm, and the thickness of the thin plate is 0.5 mm.

Citation Information

Patent Citations

  • Ceramic slurry and ceramic shell, and preparation methods thereof

    CN106495706A

  • Modification method of silicon carbide ultrafine powder and method for preparing silicon carbide ceramic by gel injection pressureless sintering

    CN116253567A

  • Processing method of water-based high-efficiency CMP (chemical mechanical polishing) pad

    CN117300922A