Yellowing-resistant polyurethane for polishing pad and preparation process thereof

By adding nano-silica and polyether polyols to the polyurethane for polishing pads, the problem of oxidation and degradation of polishing pads under ultraviolet light is solved, and its yellowing resistance and light resistance is improved, and its strength and wear resistance are enhanced. sex.

CN118027341BActive Publication Date: 2024-12-06SHANGHAI HECHENG POLYMER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410217967.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-12-06
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

The polishing pad is easily oxidized and degraded under ultraviolet light, causing yellowing and affecting its performance.

Method used

Using a yellow-resistant polyurethane for polishing pads and its preparation process, through the synthesis of prepolymers and polyurethane, nanosilica, polyether polyols and amide benzothiazole and other components are added to improve the UV resistance and light resistance of polyurethane. , and improve its strength and toughness through silanization modification and polycyclic structure.

Benefits of technology

It significantly improves the yellowing and UV resistance of the polyurethane used in polishing pads, enhances its strength and wear resistance, and extends its service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane for polishing pads, specifically to a yellowing-resistant polyurethane for polishing pads and a preparation process thereof, comprising the following preparation processes: mixing diisocyanate, polyether polyol and chain extender, slowly heating to 75-85°C, keeping warm for reaction for 2-3h to obtain prepolymer; adding nano-silicon dioxide, foaming agent, homogenizing agent and plasticizer for mixing; adding curing agent, pouring into a mold, placing at 102-108°C for thermal curing; demoulding; placing at 102-108°C for aging for 15-16h; placing at room temperature for 7d to obtain polyurethane for polishing pads. The invention introduces nadic anhydride through polyether polyol, adds caprolactam for reaction and polymerization to form a polyamide chain, so as to improve the strength, toughness, heat resistance and wear resistance of the prepared polyurethane for polishing pads; and further improves its light stability, strength and wear resistance through the amidobenzothiazole structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane for polishing pads, in particular to yellowing-resistant polyurethane for polishing pads and a preparation process thereof. Background Art

[0002] As an ultra-precision processing technology, polishing has been widely used in the processing of precision mechanical parts, precision molds, semiconductor wafers, optical components and other fields. Chemical mechanical polishing (CMP) is currently recognized as an effective surface smoothing technology, which can be applied to the polishing of metal materials such as alloys and the surface treatment of semiconductors such as silicon carbide. After the workpiece to be processed is supported, it uses the polishing liquid and chemical corrosion, and applies a certain load to contact the polishing pad to complete the removal of the workpiece surface material. As one of the important components in the polishing process, the polishing pad has the functions of storing and transporting the polishing liquid, establishing the polishing liquid circulation; removing polishing chips; removing the mechanical load of the transfer material; and maintaining the mechanical and chemical environment required for the polishing process. However, some chemical mechanical polishing uses ultraviolet light catalysis to assist, and light exposure will cause oxidation and degradation of the polishing pad, resulting in yellowing and a decrease in performance. Therefore, we propose a yellowing-resistant polyurethane for polishing pads and its preparation process. Summary of the invention

[0003] The object of the present invention is to provide a yellowing-resistant polyurethane for polishing pads and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0005] Step (1) Preparation of prepolymer:

[0006] Mix diisocyanate, polyether polyol and chain extender, slowly heat to 75-85°C, and keep warm for 2-3 hours to obtain prepolymer;

[0007] Step (2) Preparation of polyurethane:

[0008] Adjust the temperature of the prepolymer to 60-80°C, add nano-silicon dioxide, foaming agent, homogenizing agent and plasticizer, mix, stir and degas;

[0009] The mixture is mixed with a curing agent, poured into a mold, placed at a temperature of 102 to 108° C., and cured for 25 to 35 minutes; demolded; placed at a temperature of 102 to 108° C., and aged for 15 to 16 hours; and placed at room temperature for 7 days to obtain a polyurethane for a polishing pad.

[0010] Furthermore, the polyurethane for polishing pad includes the following components by mass: 20 to 40 parts of diisocyanate, 40 to 65 parts of polyether polyol, 2 to 10 parts of chain extender, 15 to 30 parts of curing agent, 0.20 to 0.27 parts of nano-silica, 0.2 to 2.0 parts of foaming agent, 0.1 to 1.0 parts of uniform foaming agent, and 6 to 10 parts of plasticizer.

[0011] Furthermore, the diisocyanate is a mixture of one or more of toluene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate.

[0012] Furthermore, the chain extender is one of diethylene glycol and 1,4-butanediol or a mixture of the two.

[0013] Furthermore, the curing agent is one or a mixture of dimethylthiotoluenediamine (DMTDA) and dichlorodiphenylmethane (MOCA); before use, preheat to 102-107° C., melt and keep warm;

[0014] The plasticizer was dibutyl phthalate (DBP), which was sourced from Sinopharm Chemical Reagent Co., Ltd.;

[0015] The blowing agent is expanding microspheres, Expancel@DU, from Akzo Nobel China;

[0016] The foaming agent is polyurethane silicone oil and L580 surfactant.

[0017] Furthermore, the nano-silicon dioxide is modified by silanization, and the specific process is as follows:

[0018] Take nano-silicon dioxide, add it to 80wt% anhydrous ethanol solution, ultrasonically disperse it for 30 minutes, heat it to 80°C, add γ-aminopropyltriethoxysilane with a mass ratio of 2 to 20% of the nano-silicon dioxide, stir and react for 2 hours; cool and filter to obtain a modified filler;

[0019] The ratio of nano-silica to anhydrous ethanol solution is 8 g / 100 mL;

[0020] Nano-silicon dioxide: particle size 20-30nm, sourced from Zhoushan Mingri Nanomaterials Co., Ltd.

[0021] In the above technical solution, nanofiller silica has good surface effect and size effect, which has a great influence on its optical properties. It can be used as a stabilizer in polyurethane to effectively inhibit the decomposition and oxidation of polyurethane under light, and improve its anti-ultraviolet and yellowing resistance. When nanofiller silica is used, it can improve the dispersibility of nanofiller in polyurethane system after surface silanization modification, and help improve the strength and toughness of polyurethane for polishing pads.

[0022] Further, the polyether polyol is prepared by the following process:

[0023] 1.1. Mix terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst in tetrahydrofuran, and heat to 40-45°C under nitrogen atmosphere, and keep constant temperature for 1-12 hours; slowly add initiator within 60 minutes, and heat to 70-75°C at a heating rate of 5°C / min, and continue to react for 3-4 hours; evaporate the solvent, cool, add dichloromethane to dissolve, ethanol to precipitate, and vacuum dry at 22-27°C for 48 hours to obtain norbornene polyether;

[0024] 1.2. Mix norbornene polyether, caprolactam, triethylamine, sodium hydride catalyst, and N-acetyl caprolactam in toluene, heat to 130-140°C under the protection of dry nitrogen atmosphere, and reflux for 8-9 hours; heat to 230-240°C and react for 18-30 minutes; add amide benzothiazole and continue to react for 8-15 minutes; cool in nitrogen to obtain polyether polyol.

[0025] Further, in step 1.1, the norbornene-based polyether includes the following components by mass: 10 parts of hydroxyl-terminated allyl polyether, 1.0 to 5.0 parts of 5-norbornene-2,3-dianhydride, 0.01 to 0.05 parts of Grubbs catalyst, and 1.1 to 1.5 parts of initiator;

[0026] The ratio of terminal hydroxyl allyl polyether and tetrahydrofuran is 5 g / 100 mL;

[0027] Terminal hydroxyl allyl polyether: E400, E450, E600, E900, relative molecular weight 400-900, from Yangzhou Chenhua Group Technology Co., Ltd.;

[0028] Grubbs catalyst: Grubbs II generation catalyst, from Anaiji Chemical;

[0029] The initiator is one of hydrogen peroxide, potassium persulfate, sodium persulfate and ammonium persulfate.

[0030] Further, in step 1.2, the polyether polyol includes the following components by mass: 10 parts of norbornene-based polyether, 5 to 10 parts of caprolactam, 0.1 to 1.0 parts of amidobenzothiazole, 0.5 to 1.0 parts of triethylamine, 0.06 to 0.08 parts of catalyst sodium hydride, and 0.15 to 0.20 parts of initiator N-acetyl caprolactam;

[0031] The ratio of norbornene polyether to toluene was 10 g / 100 mL.

[0032] Before use, caprolactam was placed at 100°C and -0.1MPa and vacuum dried for 6 hours to remove moisture.

[0033] In the above technical scheme, under the action of Grubbs catalyst and initiator, 5-norbornene-2,3-dianhydride is ring-opened and metathesized, and is polymerized with terminal hydroxyl allyl polyether through olefinic polymerization to obtain a polyether having a norbornene dianhydride structure. Then, it is mixed with caprolactam and amide-benzothiazole, caprolactam is ring-opened, reacted with the dianhydride in the norbornene-based polyether, and polymerized, and grafted with amide-benzothiazole to obtain a polyether polyol having a polyamide structure. By introducing a polyamide molecular chain into the polyether structure, the strength, toughness, heat resistance and wear resistance of the prepared polyurethane for polishing pads can be effectively improved. In addition, polycyclic structures such as norbornene and dicarboximide are introduced into the prepared polyether polyol, which not only improves the strength of the polyurethane for polishing pads, but also reduces the number of unsaturated double bonds of the benzene ring in the polyurethane system, alleviates the oxidation of the benzene ring to form a quinone structure, and helps to improve the resistance to light.

[0034] Further, amidobenzothiazole is prepared by the following process:

[0035] Dissolve cyanuric chloride in xylene, cool to 0-5°C, slowly add 2-ethylene-morpholine within 60 minutes, and then react for 100-150 minutes; add sodium hydroxide, heat to 70-75°C and react for 14 hours; extract, separate and combine the organic phases, dry over anhydrous sodium sulfate, rotary evaporate, and vacuum dry to obtain an intermediate product;

[0036] The intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide and N-methyl-1,4,7-triazabicyclodecene (MTBD) are mixed at a temperature of 50-60° C. and stirred for reaction to obtain amide benzothiazole.

[0037] Further, the molar ratio of cyanuric chloride, 2-ethylene-morpholine, and sodium hydroxide is 1:(2.0-2.1):(2.0-2.1);

[0038] Sodium hydroxide is added in the form of an aqueous solution with a concentration of 10 to 40 wt%;

[0039] The ratio of cyanuric chloride to toluene is 10 g / 100 mL.

[0040] Furthermore, the mass ratio of the intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene is 10:(12.3-13.5):(0.22-0.24).

[0041] In the above technical solution, the chlorine group in cyanuric chloride reacts with the amine group in 2-ethylene-morpholine, and multiple morpholine structures are introduced into a cyanuric chloride molecular structure by heating, and the reaction product is recorded as an intermediate product. Then, the vinyl group in the intermediate product reacts with the amine group in N-(2-aminobenzothiazole-6-yl)-acetamide to undergo a Michael addition reaction to obtain a reaction product having triazine, benzothiazole and morpholine structures, which is recorded as amide benzothiazole. Utilizing its amide structure, the above product (amide benzothiazole) is introduced into the polyurethane system structure through polyether polyols, and the benzothiazole, triazine and morpholine groups with antioxidant and light absorption capabilities can improve the light stability of the polyurethane molecular chain for the polishing pad, and its multi-ring structure can also further improve its strength and wear resistance.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1. The yellowing-resistant polyurethane for polishing pads of the present invention and its preparation process are as follows: through the preparation process of polyether polyol, nadic anhydride is introduced, and then caprolactam is added for reaction and polymerization to form a polyamide chain, so as to improve the strength, toughness, heat resistance and wear resistance of the prepared polyurethane for polishing pads; polycyclic structures such as nadic anhydride and dicarboximide can improve the strength of polyurethane for polishing pads while reducing the number of unsaturated double bonds of benzene rings in the polyurethane system, alleviating the oxidation of benzene rings to form quinone structures, and helping to improve the resistance to light.

[0044] 2. The yellowing-resistant polyurethane for polishing pads of the present invention and its preparation process, the polyether polyol also contains an amide benzothiazole structure, which is obtained by reacting cyanuric chloride, 2-ethylene-morpholine, and N-(2-aminobenzothiazole-6-yl)-acetamide, and the benzothiazole, triazine, and morpholine groups with antioxidant and light absorption capabilities are introduced into the polyurethane molecular system, which can improve the light stability of the prepared polyurethane molecular chain for polishing pads, and its multi-ring structure can also further improve its strength and wear resistance. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] In the following specific implementations,

[0047] The plasticizer was dibutyl phthalate (DBP), which was sourced from Sinopharm Chemical Reagent Co., Ltd.;

[0048] The blowing agent was foaming microspheres, Expancel@DU, 031DU 40, from Akzo Nobel China;

[0049] The foaming agent is polyurethane silicone oil and L-580 surfactant, which are from Momentive High-Tech Materials Group;

[0050] Nano-silicon dioxide: particle size 20-30nm, sourced from Zhoushan Mingri Nanomaterials Co., Ltd.

[0051] Terminal hydroxyl allyl polyether: E600, relative molecular weight 600, from Yangzhou Chenhua Group Technology Co., Ltd.;

[0052] Grubbs catalyst: Grubbs II generation catalyst, derived from Anage Chemical.

[0053] Embodiment 1: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0054] Step 1: Silanization modification of nano-silica:

[0055] Take nano-silica, add it to 80wt% anhydrous ethanol solution, ultrasonically disperse it for 30min, heat it to 80℃, add γ-aminopropyltriethoxysilane which is 2% of the mass of nano-silica, stir and react for 2h; cool and filter to obtain modified filler; the ratio of nano-silica to anhydrous ethanol solution is 8g / 100mL;

[0056] Step 2, preparation of amidobenzothiazole:

[0057] Take cyanuric chloride and dissolve it in xylene, cool it to 0°C, slowly add 2-ethylene-morpholine, add it within 60 minutes, and then react for 150 minutes; add sodium hydroxide (added in the form of 10wt% aqueous solution), heat it to 70°C and react for 14 hours; extract, separate and combine the organic phases, dry them over anhydrous sodium sulfate, rotary evaporate, and vacuum dry them to obtain an intermediate product; the molar ratio of cyanuric chloride, 2-ethylene-morpholine, and sodium hydroxide is 1:2:2; the ratio of cyanuric chloride to toluene is 10g / 100mL;

[0058] The intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene are mixed at a temperature of 50° C. and stirred for reaction to obtain amide benzothiazole; the mass ratio of the intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene is 10:12.3:0.22;

[0059] Step 3, preparation of polyether polyol:

[0060] 3.1. The terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst were mixed in tetrahydrofuran, and the temperature was raised to 40°C under nitrogen atmosphere, and the temperature was kept constant for 12 hours; potassium persulfate as an initiator was slowly added within 60 minutes, and the temperature was raised to 70°C at a heating rate of 5°C / min, and the reaction was continued for 4 hours; the solvent was evaporated, cooled, dichloromethane was added to dissolve, ethanol was precipitated, and vacuum dried at 22°C for 48 hours to obtain norbornene polyether;

[0061] The norbornene-based polyether comprises the following components by weight: 10 parts of terminal hydroxyl allyl polyether, 1.0 parts of 5-norbornene-2,3-dianhydride, 0.01 parts of Grubbs catalyst, and 1.1 parts of initiator; the ratio of terminal hydroxyl allyl polyether to tetrahydrofuran is 5 g / 100 mL;

[0062] 3.2. Caprolactam was placed at 100°C and -0.1MPa, vacuum dried for 6 hours to remove moisture; norbornene polyether, caprolactam, triethylamine, catalyst sodium hydride, initiator N-acetyl caprolactam were mixed in toluene, heated to 130°C under the protection of dry nitrogen atmosphere, and refluxed for 9 hours; heated to 230°C and reacted for 30 minutes; amidobenzothiazole was added and the reaction was continued for 15 minutes; cooled in nitrogen to obtain polyether polyol;

[0063] The polyether polyol includes the following components by mass: 10 parts of norbornene polyether, 5 parts of caprolactam, 0.1 parts of amidobenzothiazole, 0.5 parts of triethylamine, 0.06 parts of sodium hydride as a catalyst, and 0.15 parts of N-acetyl caprolactam as an initiator; the ratio of norbornene polyether to toluene is 10 g / 100 mL;

[0064] Step 4: Preparation of polyurethane:

[0065] The diisocyanate, polyether polyol and chain extender are mixed, and the temperature is slowly raised to 75°C, and the reaction is kept at this temperature for 3 hours to obtain a prepolymer; using a polyurethane high-temperature casting machine, the prepolymer is placed in a raw material tank A, and a modified filler, a foaming agent, a homogenizing agent and a plasticizer are added, and the mixture is stirred at 60r / min, vacuum degassed for 30 minutes, and kept at 60°C; the curing agent is placed in a raw material tank B, and heated to melt; the materials in the raw material tanks A and B are mixed, poured into a mold, and placed at 102°C for curing for 35 minutes; demolding; placing at 102°C for aging for 16 hours; placing at room temperature for 7 days to obtain a polyurethane for a polishing pad;

[0066] The polyurethane for polishing pad includes the following components by mass: 30 parts of diisocyanate, 40 parts of polyether polyol, 6 parts of chain extender diethylene glycol, 23 parts of curing agent dichlorodiphenylmethane, 0.20 parts of modified filler, 0.9 parts of foaming agent, 0.5 parts of uniform foaming agent, and 8 parts of plasticizer; the diisocyanate is a mixture of toluene diisocyanate and isophorone diisocyanate, with a mass ratio of 7:3.

[0067] Embodiment 2: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0068] Step 1: Silanization modification of nano-silica:

[0069] Take nano-silica, add it to 80wt% anhydrous ethanol solution, ultrasonically disperse it for 30min, heat it to 80℃, add γ-aminopropyltriethoxysilane which is 10% of the mass of nano-silica, stir and react for 2h; cool and filter to obtain modified filler; the ratio of nano-silica to anhydrous ethanol solution is 8g / 100mL;

[0070] Step 2, preparation of amidobenzothiazole:

[0071] Take cyanuric chloride and dissolve it in xylene, cool it to 2°C, slowly add 2-ethylene-morpholine, add it within 60 minutes, and then react for 120 minutes; add sodium hydroxide (added in the form of 25wt% aqueous solution), heat it to 72°C and react for 14 hours; extract, separate and combine the organic phases, dry them over anhydrous sodium sulfate, rotary evaporate, and vacuum dry them to obtain an intermediate product; the molar ratio of cyanuric chloride, 2-ethylene-morpholine, and sodium hydroxide is 1:2.05:2.05; the ratio of cyanuric chloride to toluene is 10g / 100mL;

[0072] The intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene (MTBD) are mixed at a temperature of 55° C. and stirred for reaction to obtain amide benzothiazole; the mass ratio of the intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene is 10:12.9:0.23;

[0073] Step 3, preparation of polyether polyol:

[0074] 3.1. The terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst were mixed in tetrahydrofuran, and the temperature was raised to 42°C under nitrogen atmosphere, and the temperature was kept constant for 6 hours; potassium persulfate as an initiator was slowly added within 60 minutes, and the temperature was raised to 72°C at a heating rate of 5°C / min, and the reaction was continued for 3.5 hours; the solvent was evaporated, cooled, dichloromethane was added to dissolve, ethanol was precipitated, and vacuum dried at 25°C for 48 hours to obtain norbornene polyether;

[0075] The norbornene-based polyether comprises the following components by weight: 10 parts of terminal hydroxyl allyl polyether, 3 parts of 5-norbornene-2,3-dianhydride, 0.03 parts of Grubbs catalyst, and 1.3 parts of initiator; the ratio of terminal hydroxyl allyl polyether to tetrahydrofuran is 5 g / 100 mL;

[0076] 3.2. Caprolactam was placed at 100°C and -0.1MPa, vacuum dried for 6 hours to remove moisture; norbornene polyether, caprolactam, triethylamine, catalyst sodium hydride, initiator N-acetyl caprolactam were mixed in toluene, heated to 135°C under the protection of dry nitrogen atmosphere, and refluxed for 8.5 hours; the temperature was raised to 235°C and reacted for 24 minutes; amidobenzothiazole was added and the reaction was continued for 12 minutes; and the polyether polyol was obtained by cooling in nitrogen;

[0077] The polyether polyol includes the following components by mass: 10 parts of norbornene polyether, 8 parts of caprolactam, 0.5 parts of amidobenzothiazole, 0.8 parts of triethylamine, 0.07 parts of sodium hydride as a catalyst, and 0.18 parts of N-acetyl caprolactam as an initiator; the ratio of norbornene polyether to toluene is 10 g / 100 mL;

[0078] Step 4: Preparation of polyurethane:

[0079] The diisocyanate, polyether polyol and chain extender are mixed, and the temperature is slowly raised to 80°C, and the reaction is kept at this temperature for 2.5 hours to obtain a prepolymer; using a polyurethane high-temperature casting machine, the prepolymer is placed in a raw material tank A, and a modified filler, a foaming agent, a homogenizing agent and a plasticizer are added, and the mixture is stirred at 60r / min, vacuum degassed for 30 minutes, and kept at 60°C; the curing agent is placed in a raw material tank B, and heated to melt; the materials in the raw material tanks A and B are mixed, poured into a mold, and placed at 105°C for curing for 30 minutes; demolding; placing at 105°C for aging for 15.5 hours; placing at room temperature for 7 days to obtain a polyurethane for a polishing pad;

[0080] The polyurethane for polishing pad includes the following components by mass: 30 parts of diisocyanate, 53 parts of polyether polyol, 6 parts of chain extender diethylene glycol, 23 parts of curing agent dichlorodiphenylmethane, 0.23 parts of modified filler, 1.0 parts of foaming agent, 0.5 parts of uniform foaming agent, and 8 parts of plasticizer; the diisocyanate is a mixture of toluene diisocyanate and isophorone diisocyanate, and the mass ratio is 1:1.

[0081] Embodiment 3: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0082] Step 1: Silanization modification of nano-silica:

[0083] Take nano-silica, add it to 80wt% anhydrous ethanol solution, ultrasonically disperse it for 30min, heat it to 80°C, add γ-aminopropyltriethoxysilane which is 20% of the mass of nano-silica, stir and react for 2h; cool and filter to obtain modified filler; the ratio of nano-silica to anhydrous ethanol solution is 8g / 100mL;

[0084] Step 2, preparation of amidobenzothiazole:

[0085] Dissolve cyanuric chloride in xylene, cool to 5°C, slowly add 2-ethylene-morpholine within 60 minutes, and then react for 100 minutes; add sodium hydroxide (in the form of 40wt% aqueous solution), heat to 75°C and react for 14 hours; extract, separate and combine the organic phases, dry over anhydrous sodium sulfate, rotary evaporate, and vacuum dry to obtain an intermediate product; the molar ratio of cyanuric chloride, 2-ethylene-morpholine, and sodium hydroxide is 1:2.1:2.1; the ratio of cyanuric chloride to toluene is 10g / 100mL;

[0086] The intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene (MTBD) are mixed at 60° C. and stirred for reaction to obtain amide benzothiazole; the mass ratio of the intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene is 10:13.5:0.24;

[0087] Step 3, preparation of polyether polyol:

[0088] 3.1. The terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst were mixed in tetrahydrofuran, and the temperature was raised to 45°C under nitrogen atmosphere, and the temperature was kept constant for 1 hour; the initiator sodium persulfate was slowly added within 60 minutes, and the temperature was raised to 75°C at a heating rate of 5°C / min, and the reaction was continued for 3 hours; the solvent was evaporated, cooled, and dichloromethane was added to dissolve, ethanol was precipitated, and vacuum dried at 27°C for 48 hours to obtain the norbornene polyether;

[0089] The norbornene-based polyether comprises the following components by weight: 10 parts of terminal hydroxyl allyl polyether, 5.0 parts of 5-norbornene-2,3-dianhydride, 0.05 parts of Grubbs catalyst, and 1.5 parts of initiator; the ratio of terminal hydroxyl allyl polyether to tetrahydrofuran is 5 g / 100 mL;

[0090] 3.2. Caprolactam was placed at 100°C and -0.1MPa, vacuum dried for 6 hours to remove moisture; norbornene polyether, caprolactam, triethylamine, catalyst sodium hydride, initiator N-acetyl caprolactam were mixed in toluene, heated to 140°C under the protection of dry nitrogen atmosphere, and refluxed for 8 hours; the temperature was raised to 240°C and reacted for 18 minutes; amidobenzothiazole was added and the reaction was continued for 8 minutes; and polyether polyol was obtained by cooling in nitrogen;

[0091] The polyether polyol includes the following components by mass: 10 parts of norbornene polyether, 10 parts of caprolactam, 1.0 parts of amidobenzothiazole, 1.0 parts of triethylamine, 0.08 parts of sodium hydride as a catalyst, and 0.20 parts of initiator N-acetyl caprolactam; the ratio of norbornene polyether to toluene is 10 g / 100 mL;

[0092] Step 4: Preparation of polyurethane:

[0093] The diisocyanate, polyether polyol and chain extender are mixed, and the temperature is slowly raised to 85°C, and the reaction is kept at this temperature for 2 hours to obtain a prepolymer; using a polyurethane high-temperature casting machine, the prepolymer is placed in a raw material tank A, and a modified filler, a foaming agent, a homogenizing agent and a plasticizer are added, and the mixture is stirred at 60r / min, vacuum degassed for 30 minutes, and kept at 60°C; the curing agent is placed in a raw material tank B, and heated to melt; the materials in the raw material tanks A and B are mixed, poured into a mold, and placed at 108°C for curing for 25 minutes; demolding; placing at 108°C for aging for 15 hours; placing at room temperature for 7 days to obtain a polyurethane for a polishing pad;

[0094] The polyurethane for polishing pad includes the following components by mass: 30 parts of diisocyanate, 65 parts of polyether polyol, 6 parts of chain extender diethylene glycol, 23 parts of curing agent dichlorodiphenylmethane, 0.27 parts of modified filler, 1.1 parts of foaming agent, 0.5 parts of uniform foaming agent, and 8 parts of plasticizer; the diisocyanate is a mixture of toluene diisocyanate and isophorone diisocyanate, with a mass ratio of 3:7.

[0095] Comparative Example 1: A yellowing-resistant polyurethane for a polishing pad, comprising the following components by mass: 30 parts of diisocyanate, 40 parts of polyether polyol, 6 parts of chain extender diethylene glycol, 23 parts of curing agent dichlorodiphenylamine methane, 0.9 parts of foaming agent, 0.5 parts of uniform foaming agent, and 8 parts of plasticizer; the diisocyanate is a mixture of toluene diisocyanate and isophorone diisocyanate, with a mass ratio of 7:3;

[0096] The diisocyanate, polyether polyol and chain extender are mixed, and the temperature is slowly raised to 75°C, and the reaction is kept at this temperature for 3 hours to obtain a prepolymer; using a polyurethane high-temperature casting machine, the prepolymer is placed in a raw material tank A, a foaming agent, a homogenizing agent and a plasticizer are added, and the mixture is stirred and mixed at 60r / min, vacuum degassed for 30 minutes, and kept at 60°C; the curing agent is placed in a raw material tank B, and heated to melt; the materials in the raw material tanks A and B are mixed, poured into a mold, and placed at 102°C for curing for 35 minutes; demolding; placing at 102°C for aging for 16 hours; placing at room temperature for 7 days to obtain a polyurethane for a polishing pad;

[0097] The preparation process of polyether polyol is the same as that in Example 1.

[0098] Comparative Example 2: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0099] Step 1, preparation of polyether polyol:

[0100] The terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst were mixed in tetrahydrofuran, and the temperature was raised to 40°C under the protection of nitrogen atmosphere, and the temperature was kept constant for 12 hours; the initiator potassium persulfate was slowly added, and the addition was completed within 60 minutes, and the temperature was raised to 70°C at a heating rate of 5°C / min, and the reaction was continued for 4 hours; the solvent was evaporated, cooled, and dichloromethane was added to dissolve, ethanol was precipitated, and vacuum dried at 22°C for 48 hours to obtain the norbornene-based polyether; the norbornene-based polyether includes the following mass components: 10 parts of terminal hydroxyl allyl polyether, 1.0 parts of 5-norbornene-2,3-dianhydride, 0.01 parts of Grubbs catalyst, and 1.1 parts of initiator; the ratio of terminal hydroxyl allyl polyether to tetrahydrofuran is 5g / 100mL;

[0101] Caprolactam is placed at 100°C and -0.1MPa, and vacuum dried for 6 hours to remove moisture; norbornene polyether, caprolactam, triethylamine, catalyst sodium hydride, and initiator N-acetyl caprolactam are mixed in toluene, and heated to 130°C under the protection of dry nitrogen atmosphere, and refluxed for 9 hours; the temperature is raised to 230°C and reacted for 30 minutes; the polyether polyol is cooled in nitrogen to obtain the following mass components: 10 parts of norbornene polyether, 5 parts of caprolactam, 0.5 parts of triethylamine, 0.06 parts of catalyst sodium hydride, and 0.15 parts of initiator N-acetyl caprolactam; the ratio of norbornene polyether to toluene is 10g / 100mL;

[0102] Step 2 is the same as that in Comparative Example 1 to obtain polyurethane for polishing pad.

[0103] Comparative Example 3: A preparation process of yellowing-resistant polyurethane for polishing pads, comprising the following preparation process:

[0104] The diisocyanate, polyether polyol and chain extender are mixed, and the temperature is slowly raised to 75°C, and the reaction is kept at this temperature for 3 hours to obtain a prepolymer; using a polyurethane high-temperature casting machine, the prepolymer is placed in a raw material tank A, a foaming agent, a homogenizing agent and a plasticizer are added, and the mixture is stirred and mixed at 60r / min, vacuum degassed for 30 minutes, and kept at 60°C; the curing agent is placed in a raw material tank B, and heated to melt; the materials in the raw material tanks A and B are mixed, poured into a mold, and placed at 102°C for curing for 35 minutes; demolding; placing at 102°C for aging for 16 hours; placing at room temperature for 7 days to obtain a polyurethane for a polishing pad;

[0105] The polyurethane for polishing pad includes the following components by mass: 30 parts of diisocyanate, 40 parts of polyether polyol (polytetramethylene ether glycol PTMEG1000, sourced from Gancuide (Dalian) Chemical Co., Ltd.), 6 parts of chain extender diethylene glycol, 23 parts of curing agent dichlorodiphenylmethane, 0.9 parts of foaming agent, 0.5 parts of uniform foaming agent, and 8 parts of plasticizer; the diisocyanate is a mixture of toluene diisocyanate and isophorone diisocyanate, with a mass ratio of 7:3.

[0106] Experiment: The polyurethane for polishing pad obtained in Examples 1-3 and Comparative Examples 1-3 was used to prepare samples, and the performance thereof was tested and the test results were recorded:

[0107] Mechanical properties test: GB / T 528 is used as the reference standard, and an electronic universal material testing machine is used to test the tensile strength of the polyurethane sample for polishing pads at a tensile rate of 50 mm / min.

[0108] Wear resistance test: The friction performance of the polyurethane sample for polishing pad was tested by reciprocating comprehensive tester, the experimental speed was 300r / min, the loading pressure was 10N, the running speed of the friction machine was 10mm / min, the reciprocating stroke was 5mm, the friction time was 5min, and the friction machine pressure head was a GCr15 steel ball with a diameter of 6mm;

[0109] Yellowing resistance test: Place the sample in a UV aging test box with a wavelength of 340nm, a temperature of 50℃, and irradiation for 24h. Use a colorimeter to detect the comprehensive deviation value of the sample before and after the experiment, which is recorded as the color difference.

[0110] Tensile strength(MPa) Wear rate (%) Chromatic Aberration Example 1 38 0.027 0.42 Example 2 41 0.024 0.35 Example 3 43 0.022 0.31 Comparative Example 1 34 0.034 3.93 Comparative Example 2 30 0.039 5.07 Comparative Example 3 27 0.042 6.14

[0111] According to the data in the above table, we can clearly draw the following conclusions:

[0112] The polyurethane for polishing pad obtained in Examples 1-3 is compared with the polyurethane for polishing pad obtained in Comparative Examples 1-3. The test results show that:

[0113] Compared with the comparative example, the polyurethane for polishing pad obtained in Examples 1-3 has higher tensile strength data, lower wear rate and color difference value, which fully demonstrates that the present invention achieves improvement in strength, wear resistance and yellowing resistance of the polyurethane for polishing pad.

[0114] Compared with Example 1, the nano silicon dioxide and its modified substance are not added in Comparative Example 1; compared with Comparative Example 1, the polyether polyol components in Comparative Examples 2 and 3 are different; and the tensile strength, wear rate and color difference value data thereof are deteriorated. It can be seen that the components used in the polyurethane for polishing pad and the process settings of the present invention can promote the improvement of its strength, wear resistance and yellowing resistance.

[0115] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0116] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing yellowing-resistant polyurethane for polishing pads, characterized in that: The preparation process includes the following: Step (1) Preparation of prepolymer: Mix diisocyanate, polyether polyol and chain extender, slowly heat to 75-85°C, and keep warm for 2-3 hours to obtain prepolymer; Step (2) Preparation of polyurethane: Adjust the temperature of the prepolymer to 60-80°C, add nano-silicon dioxide, foaming agent, homogenizing agent and plasticizer, mix, stir and degas; Mix with a curing agent, pour into a mold, place at 102-108° C., and cure for 25-35 minutes; demould; place at 102-108° C., and mature for 15-16 hours; place at room temperature for 7 days to obtain a polyurethane for a polishing pad; The polyether polyol is prepared by the following process: Step 1.

1. The terminal hydroxyl allyl polyether, 5-norbornene-2,3-dianhydride and Grubbs catalyst are mixed in tetrahydrofuran, and the temperature is raised to 40-45°C under the protection of nitrogen atmosphere, and the temperature is kept constant for 1-12 hours; the initiator is slowly added within 60 minutes, and the temperature is raised to 70-75°C at a heating rate of 5°C / min, and the reaction is continued for 3-4 hours to obtain the norbornene-based polyether; Step 1.

2. Mix norbornene polyether, caprolactam, triethylamine, sodium hydride catalyst, and N-acetyl caprolactam initiator in toluene, heat to 130-140° C. under dry nitrogen atmosphere, and reflux for 8-9 hours; heat to 230-240° C. and react for 18-30 minutes; add amide benzothiazole and continue to react for 8-15 minutes to obtain polyether polyol; The amide benzothiazole is prepared by the following process: Dissolve cyanuric chloride in xylene, cool to 0-5°C, slowly add 2-ethylene-morpholine within 60 minutes, and then react for 100-150 minutes; add sodium hydroxide, heat to 70-75°C, and react for 14 hours to obtain an intermediate product; The intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide and N-methyl-1,4,7-triazabicyclodecene are mixed at a temperature of 50-60° C. and stirred for reaction to obtain amide benzothiazole.

2. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 1, characterized in that: The polyurethane for polishing pad comprises the following components by mass: 20-40 parts of diisocyanate, 40-65 parts of polyether polyol, 2-10 parts of chain extender, 15-30 parts of curing agent, 0.20-0.27 parts of nano silicon dioxide, 0.2-2.0 parts of foaming agent, 0.1-1.0 parts of uniform foaming agent and 6-10 parts of plasticizer.

3. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 2, characterized in that: The diisocyanate is a mixture of one or more of toluene diisocyanate, diphenylmethane diisocyanate and isophorone diisocyanate; The chain extender is one of diethylene glycol and 1,4-butanediol or a mixture of the two; The curing agent is one of dimethylthiotoluenediamine and di-o-chlorodiphenylamine methane or a mixture of the two.

4. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 1, characterized in that: In step 1.1, the norbornene-based polyether includes the following components by weight: 10 parts of terminal hydroxyl allyl polyether, 1.0 to 5.0 parts of 5-norbornene-2,3-dianhydride, 0.01 to 0.05 parts of Grubbs catalyst, and 1.1 to 1.5 parts of initiator.

5. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 1, characterized in that: In step 1.2, the polyether polyol includes the following components by mass: 10 parts of norbornene-based polyether, 5 to 10 parts of caprolactam, 0.1 to 1.0 parts of amide benzothiazole, 0.5 to 1.0 parts of triethylamine, 0.06 to 0.08 parts of catalyst sodium hydride, and 0.15 to 0.20 parts of initiator N-acetyl caprolactam.

6. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 1, characterized in that: The molar ratio of cyanuric chloride, 2-ethylene-morpholine and sodium hydroxide is 1: (2.0-2.1): (2.0-2.1); The mass ratio of the intermediate product, N-(2-aminobenzothiazol-6-yl)-acetamide, and N-methyl-1,4,7-triazabicyclodecene is 10:(12.3-13.5):(0.22-0.24).

7. The process for preparing the yellowing-resistant polyurethane for polishing pad according to claim 1, characterized in that: The nano silicon dioxide is modified by silanization, and the specific process is as follows: Take nano-silica, add it to 80wt% anhydrous ethanol solution, ultrasonically disperse it for 30 minutes, heat it to 80°C, add γ-aminopropyltriethoxysilane in an amount of 2 to 20% by weight of the nano-silica, stir and react for 2 hours to obtain a modified filler.

8. A yellowing-resistant polyurethane for polishing pads prepared according to the preparation process according to any one of claims 1 to 7.