Preparation method of low shrinkage wafer dicing tape

By using hyperbranched macromolecules and isooctyl acrylate oligomers prepared by glucose, combined with cellulose nanocrystals, the high shrinkage and peeling residue problems of wafer cutting tape during curing are solved, and low shrinkage and high viscosity are achieved The tape preparation reduces surface stress and peeling force.

CN118027822BActive Publication Date: 2024-11-05AZUSA TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410227191.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-11-05
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Existing wafer cutting tapes will produce high shrinkage when cured, resulting in surface stress and cracks, and will easily remain during peeling.

Method used

Use glucose to prepare hyperbranched macromolecules, and combine isooctyl acrylate oligomers and cellulose nanocrystals to prepare low shrinkage wafer cutting tape, through the reaction of glucose-systopically hyperbranched macromolecules and isooctyl acrylate oligomers , improve the viscosity and peeling properties of the glue, and introduce cellulose nanocrystals to reduce peeling force.

Benefits of technology

A low shrinkage tape preparation is achieved, with no residue after the glue curing, the viscosity is improved, and the peeling force is reduced, which significantly reduces the risk of surface stress and cracks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118027822B_ABST
    Figure CN118027822B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a wafer dicing tape with low shrinkage, which specifically comprises the following steps: step 1, synthesizing glucose-based hyperbranched macromolecules; step 2, synthesizing isooctyl acrylate oligomers; and step 3, preparing a wafer dicing tape according to the products obtained in step 1 and step 2. The invention adopts glucose to prepare hyperbranched macromolecules, obtains a low-shrinkage adhesive, and leaves no residue when the adhesive is cured and peeled off. At the same time, acrylic acid is introduced into the adhesive, which not only reacts with the hyperbranched macromolecules, but also increases the viscosity of the wafer dicing adhesive; the introduction of isooctyl acrylate into the adhesive makes it easier to peel off the adhesive after curing, and the introduction of cellulose nanocrystals reduces the peeling force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of UV adhesives for electronic devices and relates to a method for preparing a low-shrinkage wafer dicing tape. Background Art

[0002] Chips, as high-end, technology-intensive products, are indispensable in many electronic products. Wafers are the most critical basic material for chips. When processing wafers, they are cut into small particles. In order to prevent flying debris from damaging the wafers during the cutting process, and to prevent adverse consequences such as edge collapse, wafer dicing tape is usually used to protect the wafers. On the one hand, the dicing tape prevents debris from flying and plays a protective role, and on the other hand, it prevents slipping edges. The dicing adhesive on the existing wafer dicing tape will reduce the distance between molecules during curing, causing the dicing adhesive to shrink in volume. The dicing adhesive itself shrinks in volume due to polymerization, which is prone to surface stress and cracks. Summary of the Invention

[0003] The purpose of the present invention is to provide a method for preparing a low-shrinkage wafer dicing tape. The wafer dicing adhesive used in the tape prepared by the method adopts glucose to prepare hyperbranched macromolecules, so that the prepared wafer dicing adhesive has the performance of low shrinkage.

[0004] The technical solution adopted by the present invention is a method for preparing a low-shrinkage wafer dicing tape, which specifically includes the following steps:

[0005] Step 1, synthesizing glucose-based hyperbranched macromolecules;

[0006] Step 2, synthesizing isooctyl acrylate oligomer;

[0007] Step 3, preparing wafer dicing tape according to the products obtained in steps 1 and 2.

[0008] The present invention is also characterized in that:

[0009] The specific process of step 1 is:

[0010] Step 1.1: Dissolve 5g-10g of glucose compound and 0.1g-0.2g of p-toluenesulfonic acid in tetrahydrofuran solvent, then add 30g-60g of 2,2-bis(hydroxymethyl)propionic acid, react at 80°C-120°C for 12h-24h, and rotary evaporate at 60-120°C to obtain the first precursor;

[0011] Step 1.2, add the first step precursor obtained in step 1.1 to 25g-50g of epichlorohydrin, add 1mL-2mL of triethylamine and stir at 45℃-90℃ for 6h-12h. After the reaction is completed, remove the unreacted raw materials by rotary evaporation at 60℃-120℃ to obtain glucose-based hyperbranched macromolecules.

[0012] The specific process of step 2 is:

[0013] 5 mL-10 mL of isooctyl acrylate was dispersed in 5 mL-10 mL of isopropanol solution, 0.001 g-0.005 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine was added, and the mixture was heated to 30°C-60°C for 1 h-3 h. After the reaction, column separation was performed using an Al2O3-filled column to obtain isooctyl acrylate oligomers.

[0014] The specific process of step 3 is:

[0015] Step 3.1: 0.8-1.6 g of glucose-based hyperbranched macromolecules, 1 g-3 g of isooctyl acrylate oligomers, 0.5-1 mL of acrylic acid, 0.2 g-0.6 g of dodecyl acrylate, 0.2 g-0.6 g of cellulose nanocrystals, and 0.1 g-0.2 g of 1-hydroxycyclohexyl phenyl ketone are sequentially added to 5 mL-10 mL of tetrahydrofuran solvent to obtain a wafer dicing glue;

[0016] Step 3.2, preparing wafer dicing tape according to the wafer dicing glue obtained in step 3.1.

[0017] The specific process of step 3.2 is:

[0018] Spread the wafer dicing glue obtained in step 3.1 on a 5cm-10cm thick polyvinyl acetate film and dry it at 45℃-60℃ for 1h-2h to obtain the product.

[0019] The present invention has the beneficial effects of using glucose to prepare hyperbranched macromolecules, resulting in a low-shrinkage adhesive that leaves no residue when the adhesive is cured and peeled. Furthermore, acrylic acid is introduced into the adhesive, which not only reacts with the hyperbranched macromolecules but also increases the viscosity of the wafer dicing adhesive. The introduction of isooctyl acrylate makes the adhesive easier to peel after curing, and the introduction of cellulose nanocrystals reduces the peeling force. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Density changes of the wafer dicing tape prepared in Example 1 and Comparative Examples 1 to 4 before and after light curing in the method for preparing the low-shrinkage wafer dicing tape of the present invention;

[0021] Figure 2 This is a comparison chart of the transparency of wafer dicing tapes prepared in Example 1 and Comparative Examples 1 to 3 in the preparation method of the low-shrinkage wafer dicing tape of the present invention. DETAILED DESCRIPTION

[0022] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0023] The method for preparing the low-shrinkage wafer dicing tape of the present invention specifically comprises the following steps:

[0024] Step 1, synthesis of glucose-based hyperbranched macromolecules, specifically:

[0025] Dissolve 5-10g of glucose compound and 0.1-0.2g of p-toluenesulfonic acid in 30mL of tetrahydrofuran solvent, then add 30-60g of 2,2-bis(hydroxymethyl)propionic acid, react at 80-120°C for 12-24h, and evaporate at 60-120°C to obtain the first precursor. Add the obtained precursor to 25-50g of epichlorohydrin, add 1-2mL of triethylamine, and stir at 45-90°C for 6-12h. After the reaction, remove the unreacted raw materials by rotary evaporation at 60-120°C to obtain the first precursor.

[0026] Step 2, the synthesis of isooctyl acrylate oligomer, is specifically:

[0027] Disperse 5-10 mL of isooctyl acrylate in 5-10 mL of isopropanol. Add 0.001-0.005 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine and heat to 30-60°C for 1-3 hours. After the reaction, separate the mixture through an Al2O3 column to obtain isooctyl acrylate oligomers.

[0028] Step 3, preparation of wafer dicing tape, specifically:

[0029] Take glucose-based hyperbranched macromolecules (0.8-1.6 g), isooctyl acrylate oligomers (1-3 g), acrylic acid (0.5-1 mL), dodecyl acrylate (0.2-0.6 g), cellulose nanocrystals (0.2-0.6 g), and 1-hydroxycyclohexyl phenyl ketone (0.1-0.2 g), and gradually add them to 5-10 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 5-10 cm polyvinyl acetate film and dried at 45-60°C for 1-2 hours to obtain the product.

[0030] Example 1

[0031] Step 1, synthesis of glucose-based hyperbranched macromolecules, specifically:

[0032] Dissolve 5g of glucose compound and 0.1g of p-toluenesulfonic acid in 30mL of tetrahydrofuran solvent, then add 30g of 2,2-bis(hydroxymethyl)propionic acid. React at 80°C for 12h, then rotary evaporate at 60°C to obtain the first-step precursor. Add the resulting precursor to 25g of epichlorohydrin, add 1mL of triethylamine, and stir at 45°C for 6h. After the reaction, remove the unreacted raw material by rotary evaporation at 60°C.

[0033] Step 2, the synthesis of isooctyl acrylate oligomer, is specifically:

[0034] Disperse 5 mL of isooctyl acrylate in 5 mL of isopropanol. Add 0.0015 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine and heat to 30°C for 1 hour. After the reaction, separate the mixture using an Al2O3 column to obtain isooctyl acrylate oligomers.

[0035] 3. Preparation of wafer dicing tape, specifically:

[0036] Take glucose-based hyperbranched macromolecules (0.8 g), isooctyl acrylate oligomers (1 g), acrylic acid (0.5 mL), dodecyl acrylate (0.2 g), cellulose nanocrystals (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), and gradually add them to 5 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 5 cm polyvinyl acetate film and dried at 45 ° C for 1 h to obtain wafer dicing tape.

[0037] Comparative Example 1 (No glucose-based hyperbranched macromolecules were added to the wafer dicing adhesive, resulting in high shrinkage after curing and residues when peeling)

[0038] 1. Synthesis of 2-ethylhexyl acrylate oligomer, specifically:

[0039] Disperse 5 mL of isooctyl acrylate in 5 mL of isopropanol. Add 0.001 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine and heat to 30°C for 1 hour. After the reaction, separate the mixture through an Al2O3-packed column to obtain isooctyl acrylate oligomers.

[0040] 2. Preparation of wafer dicing tape;

[0041] Isooctyl acrylate oligomer (1 g), acrylic acid (0.5 mL), dodecyl acrylate (0.2 g), 1-hydroxycyclohexyl phenyl ketone (0.1 g), and cellulose nanocrystals (0.2 g) were gradually added to 5 mL of tetrahydrofuran solvent to obtain wafer dicing adhesive. The adhesive was coated on a 5 cm polyethylene acetate film and dried at 45 ° C for 1 h to obtain a wafer dicing tape.

[0042] Comparative Example 2 (Isooctyl acrylate oligomer is replaced by isooctyl acrylate monomer, resulting in high viscosity, high peeling force and high shrinkage)

[0043] 1. Synthesis of glucose-based hyperbranched macromolecules, specifically:

[0044] Dissolve 5g of glucose compound and 0.1g of p-toluenesulfonic acid in 30mL of tetrahydrofuran solvent, then add 30g of 2,2-bis(hydroxymethyl)propionic acid. React at 80°C for 12h, then rotary evaporate at 60°C to obtain the first-step precursor. Add the resulting precursor to 25g of epichlorohydrin, add 1mL of triethylamine, and stir at 45°C for 6h. After the reaction, remove the unreacted raw material by rotary evaporation at 60°C.

[0045] 2. Preparation of wafer dicing tape, specifically:

[0046] Take glucose-based hyperbranched macromolecules (0.8 g), isooctyl acrylate (1 g), acrylic acid (0.5 mL), dodecyl acrylate (0.2 g), cellulose nanocrystals (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), and gradually add them to 5 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 5 cm polyvinyl acetate film and dried at 45 ° C for 1 h to obtain wafer dicing tape.

[0047] Comparative Example 3 (no acrylic acid added to the glue, low viscosity of the glue)

[0048] 1. Synthesis of glucose-based hyperbranched macromolecules, specifically:

[0049] Dissolve 5g of glucose and 0.1 part of p-toluenesulfonic acid in 30mL of tetrahydrofuran. Add 30g of 2,2-bis(hydroxymethyl)propionic acid and react at 80°C for 12h. Rotary evaporation is used to obtain the first-step precursor. This precursor is added to 25g of epichlorohydrin, followed by 1mL of triethylamine and stirring at 45°C for 6h. After the reaction, remove the unreacted raw material by rotary evaporation.

[0050] 2. Synthesis of 2-ethylhexyl acrylate oligomer, specifically:

[0051] Disperse 5 mL of isooctyl acrylate in 5 mL of isopropanol. Add 0.0015 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine and heat to 30°C for 1 hour. After the reaction, separate the mixture using an Al2O3 column to obtain isooctyl acrylate oligomers.

[0052] 3. Preparation of wafer dicing tape, specifically:

[0053] Take glucose-based hyperbranched macromolecules (0.8 g), isooctyl acrylate oligomers (1 g), dodecyl acrylate (0.2 g), cellulose nanocrystals (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), and gradually add them to 5 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 5 cm polyvinyl acetate film and dried at 45 ° C for 1 h to obtain wafer dicing tape.

[0054] Comparative Example 4 (No cellulose nanocrystals added to the glue, reduced viscosity and high light curing shrinkage)

[0055] 1. Synthesis of glucose-based hyperbranched macromolecules, specifically:

[0056] Dissolve 5g of glucose compound and 0.1g of p-toluenesulfonic acid in 30mL of tetrahydrofuran solvent, then add 30g of 2,2-bis(hydroxymethyl)propionic acid. React at 80°C for 12h, then evaporate at 60°C to obtain the first-step precursor. Add the resulting precursor to 25g of epichlorohydrin, add 1mL of triethylamine, and stir at 45°C for 6h. After the reaction, remove the unreacted raw material by evaporating at 60°C.

[0057] 2. Synthesis of 2-ethylhexyl acrylate oligomer, specifically:

[0058] Disperse 5 mL of isooctyl acrylate in 5 mL of isopropanol. Add 0.0015 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine and heat to 30°C for 1 hour. After the reaction, separate the mixture using an Al2O3 column to obtain isooctyl acrylate oligomers.

[0059] 3. Preparation of wafer dicing tape, specifically:

[0060] Take glucose-based hyperbranched macromolecules (0.8 g), isooctyl acrylate oligomers (1 g), acrylic acid (0.5 mL), dodecyl acrylate (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), and gradually add them to 5 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 5 cm polyvinyl acetate film and dried at 45 ° C for 1 h to obtain wafer dicing tape.

[0061] Test results

[0062] Table 1. Performance test results of wafer dicing adhesives in Example 1 and Comparative Examples 1-4

[0063] Shrinkage (%) Viscosity (MPa·s) Peel force (N) Peeling residue Experimental Example 1 1.3 52 15 none Comparative Example 1 14 50 16 have Comparative Example 2 10 61 21 none Comparative Example 3 9 28 9 none Comparative Example 4 13 42 13 none

[0064] Note: Shrinkage is the percentage change in volume (negative density change) of 1 mL of adhesive before and after curing. I = (M2 - M1 / M1) x 100%, where M1 is the density of the adhesive before curing and M2 is the density of the adhesive after curing. Peel strength is the force applied to the adhesive tape at 180°C in the reverse direction after UV curing on glass.

[0065] As shown in Table 1 and Figure 1As shown, glucose, as a small molecule, has multiple hydroxyl groups, each of which is grafted with a functional branched chain (alkylene oxide) to form a macromolecule, which increases the initial density of the glue and ultimately reduces the shrinkage rate of the glue. Among them, Example 1 is only 1.3%; the shrinkage rate of Comparative Example 3 is lower than that of Comparative Examples 1, 2, and 4. This is because Comparative Example 3 lacks acrylic acid monomers, which avoids the polymerization of monomers through covalent bonds and the volume shrinkage caused by the reduction of the distance between monomers. Since the hyperbranched macromolecular structure of glucose is introduced in Example 1, on the one hand, the glucose molecules do not have strong chromophores and chromophores, which gives the glue high transparency, as shown in the figure. Figure 2 shown.

[0066] In Comparative Example 1, no glucose hyperbranched macromolecules were added. After curing, the isooctyl acrylate oligomer, acrylic acid, and dodecyl acrylate were all linear polymers, failing to form crosslinks. When the glue was peeled, the linear polymer chains easily shifted in center of gravity, ultimately leaving glue residue.

[0067] In Comparative Example 2, the isooctyl acrylate oligomer was replaced with isooctyl acrylate monomer. Because the isooctyl acrylate oligomer itself has a higher density, while the isooctyl acrylate monomer has a lower density, the adhesive prepared using the isooctyl acrylate oligomer exhibits a higher initial density and exhibits minimal density change after curing. In contrast, the isooctyl acrylate monomer exhibits a lower initial density and exhibits a significant density change after curing, ultimately leading to a high shrinkage rate for the isooctyl acrylate monomer, which is unfavorable for its application. Furthermore, the polymerization of the isooctyl acrylate monomer with other monomers occurs via free radical polymerization, resulting in a disordered arrangement of the different monomers, leading to high viscosity and high peel strength.

[0068] In Comparative Example 3, the absence of acrylic acid resulted in a lower cure shrinkage, primarily due to the avoidance of volume shrinkage caused by covalent bonding during polymerization of acrylic acid monomers. The lack of hydrogen bonding between acrylic molecules and between acrylic acid and cellulose nanocrystals in the adhesive reduced viscosity and, consequently, peel strength.

[0069] In Comparative Example 4, the absence of cellulose nanocrystals resulted in a larger shrinkage rate and a lower viscosity. This is mainly because cellulose nanocrystals are crystalline polymers formed by the dense accumulation of glucose macromolecular chains, and are primarily uncrystallized polymers. Therefore, the glue hardly experiences volume shrinkage after light curing. In contrast, without the addition of cellulose nanocrystals, all other components experience volume shrinkage, resulting in a relatively large overall shrinkage rate. Failure to form hydrogen bonds between acrylic acid and nanocellulose results in a relatively lower viscosity.

[0070] Example 2

[0071] Step 1, synthesis of glucose-based hyperbranched macromolecules, specifically:

[0072] Dissolve 10g of glucose compound and 0.2g of p-toluenesulfonic acid in 30mL of tetrahydrofuran solvent, then add 60g of 2,2-bis(hydroxymethyl)propionic acid. React at 120°C for 24h. Rotary evaporation at 120°C yields the first-step precursor. Add the resulting precursor to 50g of epichlorohydrin, add 2mL of triethylamine, and stir at 90°C for 12h. After the reaction, remove unreacted material by rotary evaporation at 120°C.

[0073] Step 2, the synthesis of isooctyl acrylate oligomer, is specifically:

[0074] Disperse 10 mL of isooctyl acrylate in 10 mL of isopropanol. Add 0.001 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine. Heat to 60°C and react for 3 hours. After the reaction, separate the mixture using an Al2O3 column to obtain isooctyl acrylate oligomers.

[0075] 3. Preparation of wafer dicing tape, specifically:

[0076] Take glucose-based hyperbranched macromolecules (1.6 g), isooctyl acrylate oligomers (3 g), acrylic acid (1 mL), dodecyl acrylate (0.6 g), cellulose nanocrystals (0.6 g), and 1-hydroxycyclohexyl phenyl ketone (0.2 g), and gradually add them to 10 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on a 10 cm polyvinyl acetate film and dried at 60 ° C for 2 h to obtain wafer dicing tape.

[0077] Example 3

[0078] Step 1, synthesis of glucose-based hyperbranched macromolecules, specifically:

[0079] 8g of glucose compound and 0.15g of p-toluenesulfonic acid were dissolved in 30mL of tetrahydrofuran solvent. 50g of 2,2-bis(hydroxymethyl)propionic acid was then added. The mixture was reacted at 100°C for 20h. The precursor was then rotary evaporated at 100°C to obtain the first-step precursor. The precursor was added to 40g of epichlorohydrin, followed by 1.5mL of triethylamine and stirred at 50°C for 10h. After the reaction, the unreacted raw material was removed by rotary evaporation at 100°C.

[0080] Step 2, the synthesis of isooctyl acrylate oligomer, is specifically:

[0081] 8 mL of isooctyl acrylate was dispersed in 8 mL of isopropanol solution. 0.005 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine was added and the mixture was heated to 40°C for 2 hours. After the reaction, the mixture was separated by column separation using an Al2O3-packed column to obtain isooctyl acrylate oligomers.

[0082] 3. Preparation of wafer dicing tape, specifically:

[0083] Take glucose-based hyperbranched macromolecules (1.2 g), isooctyl acrylate oligomers (2 g), acrylic acid (0.8 mL), dodecyl acrylate (0.4 g), cellulose nanocrystals (0.4 g), and 1-hydroxycyclohexyl phenyl ketone (0.15 g), and gradually add them to 8 mL of tetrahydrofuran solvent to obtain wafer dicing glue. The glue is coated on an 8 cm polyvinyl acetate film and dried at 50°C for 1.5 h to obtain a wafer dicing tape.

Claims

1. A method for preparing a low shrinkage wafer dicing tape, characterized in that: The specific steps include: Step 1, synthesizing glucose-based hyperbranched macromolecules; The specific process of step 1 is as follows: Step 1.1, 5g-10g of glucose compound and 0.1g-0.2g of p-toluenesulfonic acid are dissolved in tetrahydrofuran solvent, and then 30g-60g of 2,2-bis(hydroxymethyl)propionic acid is added, reacted at 80°C-120°C for 12h-24h, and rotary evaporated at 60-120°C to obtain the first step precursor; Step 1.2, adding the first step precursor obtained in step 1.1 to 25g-50g of epichlorohydrin, adding 1mL-2mL of triethylamine and stirring at 45℃-90℃ for 6h-12h, after the reaction is completed, removing the unreacted raw materials by rotary evaporation at 60℃-120℃ to obtain glucose-based hyperbranched macromolecules; Step 2, synthesizing isooctyl acrylate oligomer; The specific process of step 2 is: 5 mL-10 mL of isooctyl acrylate is dispersed in 5 mL-10 mL of isopropanol solution, 0.001 g-0.005 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine is added, and the mixture is heated to 30°C-60°C for reaction for 1 h-3 h. After the reaction is completed, column separation is performed through an Al2O3 filled column to obtain isooctyl acrylate oligomers; Step 3, preparing wafer dicing tape according to the products obtained in step 1 and step 2.

2. The method for preparing the low shrinkage wafer dicing tape according to claim 1, characterized in that: The specific process of step 3 is as follows: Step 3.1, take 0.8g-1.6g of glucose-based hyperbranched macromolecules, 1g-3g of isooctyl acrylate oligomers, 0.5-1mL of acrylic acid, 0.2g-0.6g of dodecyl acrylate, 0.2g-0.6g of cellulose nanocrystals, and 0.1g-0.2g of 1-hydroxycyclohexyl phenyl ketone, and add them sequentially into 5mL-10mL of tetrahydrofuran solvent to obtain wafer dicing glue; Step 3.2, preparing wafer dicing tape according to the wafer dicing glue obtained in step 3.

1.

3. The method for preparing the low shrinkage wafer dicing tape according to claim 2, characterized in that: The specific process of step 3.2 is as follows: Spread the wafer dicing glue obtained in step 3.1 on a 5cm-10cm thick polyvinyl acetate film and heat at 45 o C-60 o C for 1h-2h to obtain.