Modified wool fiber, preparation method, composite water-based resin and preparation method thereof
By surface etching and chemical modification of wool fibers, the problem of insufficient mechanical properties and permeability of water-based resins is solved, and the efficient combination of wool fibers and water-based resins is achieved, which significantly improves the mechanical properties and permeability of composite materials. and flame retardant properties.
Patent Information
- Application Number
- CN202410437742.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-04-12
AI Technical Summary
Water-based resins have shortcomings in mechanical properties, thermal stability and permeability, and wool fibers fail to effectively enhance their performance, mainly due to the weak interface between the fiber and the resin.
The surface etching of wool fibers is increased by sodium hypochlorite and ozone, and chemically modified with titanate coupling agent to improve the interface compatibility between the fiber and the aqueous resin, forming mechanical interlocking and covalent bond synergy It can improve mechanical properties, permeability and flame retardant properties.
The mechanical properties, permeability and flame retardant properties of aqueous resins are significantly improved. Through the combination of physical modification and chemical modification, the interface compatibility and dispersion between fibers and resins are enhanced to form a high-performance composite material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-based resin composite materials, and in particular relates to modified wool fiber, a preparation method, a composite water-based resin and a preparation method thereof. Background Art
[0002] Waterborne resins have poor water and air permeability, and are prone to yellowing and degradation under light, resulting in decreased mechanical properties and thermal stability, so their applications are limited. In order to improve the mechanical properties, thermal stability, and water and air permeability of waterborne resins, different functional fillers can be added to them to prepare composite materials. For example, graphene, carbon nanotubes, montmorillonite, kaolin, nano dioxide, cellulose, lignin, and dopamine can improve the mechanical properties and thermal stability of waterborne resins. However, due to the limitations of development costs, preparation processes, and product performance, it is still extremely challenging to simultaneously improve the above properties of composite materials.
[0003] Wool is a high-value-added natural fiber with a unique structure, good biocompatibility and biological activity. It has excellent elasticity, hygroscopicity and low thermal conductivity, as well as good insulation ability, affinity with dyes, is non-toxic and skin-friendly, and does not produce plastic particle pollution. As a representative of protein fiber, wool is widely used in the textile and garment industry.
[0004] There is no report on using wool fiber to enhance the mechanical properties, water vapor permeability and flame retardancy of water-based resins. Before the mercerization process, the outer surface of wool fiber has a dense and smooth scale layer, which leads to a weak interface between the fiber and the water-based resin and poor mechanical properties.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The present invention aims to solve at least one of the above technical problems and proposes modified wool fiber, a preparation method, a composite water-based resin and a preparation method thereof.
[0007] To achieve the above objectives, the present invention provides the following technical solutions.
[0008] The first technical solution provided by the present invention is a method for preparing modified wool fibers, which comprises using sodium hypochlorite and ozone to simultaneously etch the surface of pretreated wool fibers at pH 4.5-5.5 for 10-100 minutes, followed by washing and drying.
[0009] Preferably, the pretreatment is to crush the wool fibers into 20-200 meshes.
[0010] Preferably, the concentration of the sodium hypochlorite is 0.2-4 g / L.
[0011] The second technical solution provided by the present invention is a preparation method of combined modified wool fiber. After the preparation method of the modified wool fiber in the first technical solution, a titanate coupling agent solution is added, reacted at room temperature for 1-2 hours, and then washed and dried.
[0012] Preferably, the titanate coupling agent is used in an amount of 0.3%-3% of the mass of the wool fiber.
[0013] Preferably, the titanate coupling agent comprises tetraisopropyl di(dioctylphosphite) titanate, a chelate solution of ethylene titanate and triethanolamine, and a chelate 100 type titanate coupling agent.
[0014] The third technical solution provided by the present invention is the modified wool fiber obtained according to the first technical solution.
[0015] The fourth technical solution provided by the present invention is the combined modified wool fiber obtained according to the second technical solution.
[0016] The fifth technical solution provided by the present invention is a composite water-based resin, which comprises the modified wool fiber of the third technical solution and a water-based resin; the mass ratio of the modified wool fiber to the water-based resin is 1:1-1:20; the water-based resin comprises any one or more of a water-based polyurethane resin, a water-based polyester resin, a silicone resin and a water-based acrylic resin.
[0017] The sixth technical solution provided by the present invention is the preparation method of the composite water-based resin in the fifth technical solution, wherein the modified wool fiber is blended with the water-based resin, stirred at a rate of 200-800 r / min at room temperature for 10-30 min, and then dried.
[0018] Preferably, the drying temperature is 90°C-103°C.
[0019] The seventh technical solution provided by the present invention is a composite water-based resin, which comprises the combined modified wool fiber and water-based resin of the fourth technical solution; the mass ratio of the modified wool fiber to the water-based resin is 1:1-1:20; the water-based resin comprises any one or more of water-based polyurethane resin, water-based polyester resin, silicone resin and water-based acrylic resin.
[0020] The eighth technical solution provided by the present invention is the preparation method of the composite water-based resin in the seventh technical solution, wherein the modified wool fiber is blended with the water-based resin, stirred at a rate of 200-800 r / min at room temperature for 10-30 min, and then dried.
[0021] Preferably, the drying temperature is 90°C-103°C.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention uses sodium hypochlorite and ozone to etch the surface of wool fibers to achieve physical modification, which can increase the surface roughness of the wool. When the wool is subsequently compounded with a water-based resin, mechanical interlocking can be generated with the surface of the water-based resin, thereby improving the mechanical properties of the water-based resin.
[0024] The invention adopts titanate coupling agent to perform surface modification on the basis of physically modified wool fiber, thereby increasing the chemical activity on the surface of the wool fiber, improving the dispersibility of the wool fiber in the resin, and enhancing the interface compatibility between the wool fiber and the water-based resin.
[0025] After the wool fiber physically modified by surface etching is compounded with the water-based resin, the physical and mechanical interlocking between the wool fiber surface and the water-based resin interface can be achieved, thereby improving the mechanical properties, water permeability and flame retardancy of the water-based resin.
[0026] After the combined modified wool fiber subjected to surface etching physical modification and titanate coupling agent treatment is compounded with a water-based resin, the mechanical properties, water permeability and flame retardancy of the water-based resin are further improved through physical mechanical interlocking and covalent bond synergy at the interface between the fiber and the water-based resin. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments.It should be understood that these descriptions are exemplary only, and are not intended to limit the scope of the present invention.In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.Unspecified conditions in the embodiments are carried out according to the conditions of normal conditions or manufacturer recommendations.Reagents used or instruments that do not specify manufacturers are conventional products that can be purchased and obtained commercially.
[0028] The first embodiment of the present invention provides a method for preparing modified wool fiber, wherein the pretreated wool is surface-etched by sodium hypochlorite and ozone at pH 4.5-5.5 for 10-100 minutes, followed by washing and drying.
[0029] In some preferred embodiments, the pretreatment is to crush the wool fibers into 20-200 meshes.
[0030] The invention pulverizes wool fibers to homogenize the wool fibers. Controlling the particle size after pulverization within this range can control the fiber aspect ratio and enhance the mechanical properties of the water-based resin.
[0031] The embodiment of the present invention etches the wool fiber surface by sodium hypochlorite and ozone, that is, physically modifies the wool fiber, which can increase the surface roughness of the wool, and then when it is subsequently compounded with a water-based resin, it can generate mechanical interlocking with the surface of the water-based resin.
[0032] The amount of sodium hypochlorite used is suitable for opening the wool fiber scales but not falling off. In some preferred embodiments, the concentration of sodium hypochlorite can be 0.2-4 g / L, for example, 0.2 g / L, 1 g / L, 2 g / L, 4 g / L, etc.
[0033] The washing refers to washing the surface-etched solid material, i.e., wool fiber, with water to remove unreacted sodium hypochlorite; then the solid material is dried, and the drying temperature and time are selected according to the amount of the solid material, for example, it can be dried at 80±2°C for 24 hours.
[0034] In some preferred embodiments, the mass flow rate of ozone is 30-150 g / h.
[0035] The second embodiment of the present invention provides a method for preparing combined modified wool fibers, which is further chemically modified after the first embodiment. Specifically, after the preparation method of the modified wool fibers in the first embodiment, a titanate coupling agent solution is added, reacted at room temperature for 1-2 hours, and then washed and dried.
[0036] The embodiment of the present invention performs chemical modification on the basis of physically modified wool fibers, which can increase the active sites on the surface of the wool fibers and improve the interface compatibility between the wool and the resin.
[0037] There is no special limitation on the dosage and specific composition of the titanate coupling agent, and those skilled in the art can adjust the dosage of the coupling agent according to the modified object and the specific type of coupling agent. For example, in some preferred embodiments, the dosage of the coupling agent is 0.3%-3% of the mass of the wool fiber.
[0038] In some preferred embodiments, the titanate coupling agent may include tetraisopropyl di(dioctylphosphite) titanate, a chelate solution of ethylene titanate and triethanolamine, or a chelate 100 type titanate coupling agent.
[0039] The water washing and drying refers to washing the solid material modified by the titanate coupling agent, i.e. the wool fiber, with water to remove the unreacted titanate coupling agent; then drying the solid material, and the drying temperature and time are selected according to the amount of the solid material, for example, it can be dried at 80±2°C for 24h.
[0040] The third embodiment of the present invention provides the modified wool fiber obtained according to the first technical solution.
[0041] The fourth embodiment of the present invention provides a combined modified wool fiber obtained according to the second technical solution.
[0042] The fifth embodiment of the present invention provides a composite water-based resin, comprising the modified wool fiber of the third technical solution and a water-based resin, wherein the mass ratio of the modified wool fiber to the water-based resin is 1:1-1:20; the water-based resin comprises a water-based polyurethane resin, a water-based polyester resin, a silicone resin and a water-based acrylic resin.
[0043] The modified wool fiber in the embodiment of the present invention has a rough surface, so when it is compounded with the water-based resin, a physical and mechanical lock can be formed at the interface between the modified wool fiber and the water-based resin, thereby improving the mechanical properties of the polyurethane. At the same time, due to the good water permeability and surface hydrophilicity of the wool itself, as well as its uniform dispersion in the resin matrix, a continuous water permeability passage is formed in the composite material, so the water permeability is significantly improved. In addition, the nitrogen content in the wool fiber is relatively high, and the flame-retardant nitrogen-containing compounds produced during the high-temperature decomposition process can dilute the concentration of the combustion gas near the flame. After compounding it with the water-based resin, the flame retardant effect of the water-based resin can be improved.
[0044] The sixth embodiment of the present invention provides a composite water-based resin, comprising the combined modified wool fiber and water-based resin of the fourth technical solution, wherein the mass ratio of the modified wool fiber to the water-based resin is 1:1-1:20; the water-based resin comprises any one or more of water-based polyurethane resin, water-based polyester resin, silicone resin and water-based acrylic resin.
[0045] After the modified wool fiber in the embodiment of the present invention is surface etched and modified with a titanate coupling agent, the surface roughness and reactivity of the wool fiber are significantly enhanced. When it is compounded with a water-based resin, the mechanical properties of the water-based resin are further improved through the physical and mechanical interlocking and covalent bond synergy between the fiber and the water-based resin interface. At the same time, due to the good water permeability and surface hydrophilicity of the wool itself, as well as its uniform dispersion in the resin matrix, a continuous water permeability passage is formed in the composite material, so the water permeability is significantly improved. In addition, the nitrogen content in the wool fiber is relatively high, and the flame-retardant nitrogen-containing compounds produced during the high-temperature decomposition process can dilute the concentration of the combustion gas near the flame. After compounding it with the water-based resin, the flame retardant effect of the water-based resin can be improved.
[0046] The seventh embodiment of the present invention provides a method for preparing a composite water-based resin, that is, the method for preparing a composite water-based resin in the fifth embodiment and the sixth embodiment. The two preparation methods are the same, specifically comprising blending the modified wool fiber / combined modified wool fiber with the water-based resin, stirring the mixture at a rate of 200-800 r / min at room temperature for 10-30 min, and then drying the mixture.
[0047] There is no need to specifically limit the drying temperature and time, and those skilled in the art can adjust them adaptively according to the needs of the final product. For example, in some preferred embodiments, the drying temperature can be 90-103°C.
[0048] In order to make the technical solution of the present invention clearer, the preparation method, application and performance of the modified wool fiber are described in detail through multiple specific embodiments below.
[0049] Some of the substance information used in the specific embodiments of the present invention may be as follows:
[0050] Waste wool fiber, sourced from Xinji Baolong Technology Co., Ltd.;
[0051] Water-based polyurethane: model KT702, manufacturer: Hefei Ketian Water-based Technology Co., Ltd.; but not limited to this.
[0052] The wool fibers used in the following specific embodiments can be prepared from wool waste (but not limited thereto), and the specific preparation method can be referred to as follows:
[0053] The waste wool is pulverized using a pulverizer with a cooling device or an air dispersion device, and passed through a 40-mesh sieve to obtain wool fibers through pretreatment.
[0054] Example 1
[0055] This embodiment provides a method for preparing modified wool fiber, comprising the following steps:
[0056] (1) Place 80 g of sodium hypochlorite in 80 L of room temperature water, stir evenly to prepare a treatment solution with a concentration of 1 g / L, and set aside.
[0057] (2) Take 4 kg of wool fiber and place it in a container. Add the above treatment solution and use an ozone generator to introduce ozone into the container. Stir to evenly disperse the fiber in the water. Adjust the pH to 4.5 and stir for 30 minutes to obtain an aqueous dispersion of wool fiber. Filter and wash the solid material with water. Repeat this process 3 times to remove unreacted sodium hypochlorite. Then dry the solid material at 80±2℃ for 24 hours to obtain surface-etched wool fiber.
[0058] (3) 4 kg of wool fiber after surface etching was added to 40 L of water, and 80 g of a chelate solution of ethylene titanate and triethanolamine (2% of the mass of the wool fiber) was added to obtain a mixture; then the pH of the mixture was adjusted to 7-8 with a 0.1 mol / L aqueous solution of sodium bicarbonate and kept stable, and after mechanical stirring for 1 h, the mixture was filtered and the solid material was washed with water, and the process was repeated 3 times to remove the unreacted coupling agent; then the solid material was dried at 80±2°C for 24 h to obtain modified wool fiber.
[0059] Example 2
[0060] This example is based on the preparation method of Example 1, except that:
[0061] In step (1), the concentration of the treatment solution is 0.2 g / l.
[0062] Example 3
[0063] This example is based on the preparation method of Example 1, except that:
[0064] In step (1), the concentration of the treatment solution is 4 g / l.
[0065] Example 4
[0066] This example is based on the preparation method of Example 1, except that:
[0067] In step (3), the amount of titanate coupling agent used is 0.3% of the mass of the wool fiber.
[0068] Example 5
[0069] This example is based on the preparation method of Example 1, except that:
[0070] In step (3), the amount of titanate coupling agent used is 3%.
[0071] Example 6
[0072] This example is based on the preparation method of Example 1, except that:
[0073] In step (3), the titanate coupling agent used is bis(dioctyl pyrophosphate)hydroxyacetate titanate.
[0074] Example 7
[0075] This example is based on the preparation method of Example 1, except that:
[0076] Step (3) is eliminated, that is, the surface-etched wool fiber is prepared according to steps (1)-(2).
[0077] Embodiment 8-15
[0078] Examples 8-15 provide different composite water-based resins and preparation methods thereof. The raw material formula of the composite water-based resin is shown in Table 1 below.
[0079] Table 1 Raw material ratios of different composite water-based resins
[0080] .
[0081] The preparation method of the composite water-based resin of Examples 8-15 comprises the following steps:
[0082] The modified wool fiber and the waterborne polyurethane material were blended in the above proportions, stirred at a rate of 500 r / min at room temperature for 10 min, poured into a polytetrafluoroethylene mold, placed in an oven at 100±3°C, and taken out after drying to obtain a composite waterborne resin material.
[0083] Comparative Example 1
[0084] Comparative Example 1 refers to the preparation method of Example 8, except that the modified wool fiber of Example 8 is replaced by an equal amount of unmodified wool fiber.
[0085] Comparative Example 2
[0086] This example refers to the preparation method of Example 8, with the only difference being that only the wool fiber is directly treated with the titanate coupling agent.
[0087] Experimental Example 1
[0088] In order to compare and illustrate the tensile strength of the composite water-based resins of the embodiments of the present invention and the comparative examples, the tensile properties of the materials of embodiments 8-15 and comparative examples 1-2 were tested with reference to the ASTM D412 standard. The test results are shown in Table 2.
[0089] Table 2 Tensile strength test results of different composite waterborne resins
[0090] .
[0091] Experimental Example 2
[0092] In order to compare and illustrate the water-based composite resins of various embodiments of the present invention and comparative examples, the water-based composite resins of embodiments 8-15 and comparative examples 1-2 were tested for their water-based composite resins with reference to the QBT1811-1993 standard. The test results are shown in Table 3.
[0093] Table 3 Water permeability test results of different composite water-based resins
[0094] .
[0095] Experimental Example 3
[0096] In order to compare and illustrate the flame retardant properties of the composite water-based resins of the embodiments of the present invention and the comparative examples, the flame retardant properties of the materials of embodiments 8-15 and comparative examples 1-2 were tested with reference to the ASTM D2863-77 standard. The test results are shown in Table 4.
[0097] Table 4 Flame retardant test results of different composite water-based resins
[0098] .
[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite water-based resin, characterized in that: It comprises a combined modified wool fiber and a water-based resin, wherein the mass ratio of the modified wool fiber to the water-based resin is 1:1-1:20; The water-based resin is a water-based polyurethane resin; The preparation method of the combined modified wool fiber comprises the following steps: using sodium hypochlorite and ozone to simultaneously etch the surface of the pretreated wool fiber at pH 4.5-5.5 for 10-100 minutes, adding a titanate coupling agent solution, reacting at room temperature for 1-2 hours, and then washing and drying.
2. The composite water-based resin according to claim 1, characterized in that The concentration of the sodium hypochlorite is 0.2-4 g / L.
3. The composite water-based resin according to claim 1, characterized in that The dosage of titanate coupling agent is 0.3%-3% of the wool fiber mass.
4. The method for preparing the composite water-based resin according to any one of claims 1 to 3, characterized in that: The combined modified wool fiber and the water-based resin are blended and stirred at a rate of 200-800 r / min for 10-30 minutes at room temperature, and then dried.
Citation Information
Patent Citations
High temperature resistant plant fiber composite material
CN108752642A
Continuous processing method and device for improving fulling resistance of wool fabric
CN113430815A