A method for preparing a catalytic fiber and a catalytic filter bag for removing dioxins, NOx and dust from flue gas at low temperature
By using raw materials such as titanium dioxide to prepare catalytic fibers and filter bags that combine catalyst powder with PTFE resin, the efficient removal of dioxin, NOx and dust in low-temperature flue gas is solved, and efficient coordinated treatment of multiple pollutants is achieved, and the improvement of the efficient coordinated treatment of multiple pollutants is achieved. The stability and service life of the catalyst are achieved.
Patent Information
- Application Number
- CN202410183176.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-02-19
AI Technical Summary
The prior art is difficult to efficiently remove dioxin, NOx and dust in flue gas under low temperature conditions, and the activity of the catalyst is easily reduced in high SO2 and HCl environments and has a short service life.
The catalyst powder is prepared by ball milling by using raw materials such as titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate, and combined with PTFE resin and lubricant. It is prepared by ultrasonic shock and drying treatment to prepare high-active and stable catalytic fibers and catalytic filter bags are used for low-temperature flue gas treatment.
The efficient low-temperature removal of dioxin, NOx and dust is achieved. The catalytic filter bag has a dioxin removal efficiency of 98.72%, the NOx removal efficiency is 99.54%, and the dust filtration efficiency is 99.97%, and the service life is long. Good stability.
Smart Images

Figure CN118048707B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical industry, and specifically relates to a method for preparing a catalytic fiber and a catalytic filter bag for removing dioxins, NOx and dust from flue gas at low temperature. Background Art
[0002] There are two main types of dioxin emission control methods: one is dioxin generation inhibition, and the other is tail removal of generated dioxins. Dioxin generation inhibition includes methods of reducing the generation of incomplete combustion products by optimizing the combustion conditions during incineration, and methods of inhibiting dioxin generation by adding some sulfur-based or nitrogen-based compounds. The above methods are limited in their effectiveness in controlling dioxin emissions only through dioxin generation inhibition, so it is also necessary to use terminal control measures to achieve efficient removal of dioxins.
[0003] In recent years, activated carbon adsorption has been widely used for dioxin terminal control. However, activated carbon adsorption can only achieve the transfer of dioxin pollution from the gas phase to the solid phase, but cannot achieve the complete degradation of dioxins. In order to completely mineralize dioxins and form inorganic small molecules such as CO2, H2O, HCl, etc. without causing secondary pollution, it is necessary to catalytically degrade them. Catalytic degradation is considered to be the most promising dioxin terminal control technology.
[0004] Dust filter bags are widely used in the removal of particulate matter in the flue gas of garbage incineration. The removal efficiency of dust bag dust collectors can reach more than 99.9%. If catalytic filter bags can be used to remove particulate matter, dioxins and NOx in an integrated manner, it will not only be possible to achieve multiple functions on the same product to achieve multi-pollutant-free coordinated treatment, but also to replace the dust filter bags with catalytic filter bags without increasing equipment investment. In the process of dust removal at the end of the flue gas, pollutants can also be degraded into low-toxic organic matter and non-toxic inorganic small molecules to be discharged into the environment without causing secondary pollution.
[0005] The technology of integrated catalytic filter bag for removing particulate matter, dioxin and NOx mainly includes two aspects: on the one hand, the research of dioxin low temperature catalyst; on the other hand, the research of organic combination of filter material and catalyst. The incineration flue gas has complex components, high SO2 and HCl content, and high humidity, which can easily lead to catalyst poisoning and loss of activity, directly affecting the catalytic activity and service life of the catalyst. Therefore, it is very necessary to develop a catalyst formula with high catalytic activity and prepare a catalytic product with long service life. Summary of the invention
[0006] In order to solve at least one of the above problems, the present invention provides a method for preparing a catalytic fiber and a catalytic filter bag for removing dioxins, NOx and dust from flue gas at low temperature. The dioxin catalytic fiber and catalytic filter bag of the present invention can be mass-produced, reduce costs, have a wide applicable temperature range, and have a long service life, and have good application prospects.
[0007] In order to achieve the above object, the present invention adopts the following technical means:
[0008] The first aspect of the present invention provides a method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature, comprising the following steps:
[0009] (1) preparing catalyst powder: using titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate, and cerium nitrate as raw materials, and doping by ball milling to obtain catalyst powder;
[0010] (2) Surface modification of catalyst powder: Add the catalyst powder to the highly concentrated PTFE resin emulsion, with the mass ratio of catalyst to PTFE emulsion being 1:3-1:6, and the ultrasonic frequency being 10-30kHz and the oscillation time being 20-40min, and then put into an oven to dry at 60-80°C;
[0011] (3) Preparing catalytic fibers: uniformly mixing the catalyst powder surface-modified in step (2) with the organic polymer resin powder, adding lubricants and additives and mixing for 25-35 minutes, standing at 20-40°C for 72-120 hours, and then standing at 40-80°C for 12-24 hours to mature; the mixed material is pressed into a billet at 20-30°C, and then extruded and calendered at 40-60°C to form a base tape, degreased and stretched at 180-300°C to form a degreased base tape, and heat-set at 320-420°C for 20-80 seconds to form a sintered base tape, which is then opened on a fiber opening device to obtain catalytic fibers.
[0012] In some embodiments of the present invention, in the raw materials, the mass ratio of titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate is: (8-12): (0.8-1.2): (0.4-0.6): (0.4-0.6): (0.08-0.12).
[0013] In some embodiments of the present invention, the preparation process of the catalyst powder is: ball-to-material mass ratio (5-30): 1, rotation speed 400-800r / min, ball milling time 2-10h, and the obtained powder is calcined in an air atmosphere at 400-600℃ for 3-6h. In some specific embodiments, the air atmosphere, the heating rate is 5℃ / min. Further, in the ball mill, the diameters of the zirconium oxide balls are 10mm and 5mm, and the mass ratio of large balls to small balls is 1:1.
[0014] In some embodiments of the present invention, the mass ratio of the catalyst powder to the organic polymer resin powder is 1:(9-100).
[0015] In some embodiments of the present invention, the mass ratio of the organic polymer resin powder to the lubricant is (4-5):1.
[0016] In some embodiments of the present invention, the lubricant used is one of the liquid solvent petroleum ether, kerosene, and paraffin; and the additive is one of aluminum oxide and aluminum.
[0017] In some embodiments of the present invention, the organic polymer resin powder is one of polytetrafluoroethylene, polyphenylene sulfide, and polyimide. Preferably, the organic polymer resin powder is polytetrafluoroethylene.
[0018] In some embodiments of the present invention, the organic polymer resin powder has a crystallinity of more than 99%.
[0019] The second aspect of the present invention provides a catalytic filter bag, wherein the catalytic filter bag is prepared by the catalytic fiber prepared by the method described in any one of claims 1 to 8, and the needle-punched felt is obtained by coarse opening, cotton mixing box, fine opening, air pressure cotton box, carding machine, cross-lapping machine, pre-needling, main needling, trimming and winding, and the needle-punched felt is obtained by impregnation, drying, coating and sewing.
[0020] The third aspect of the present invention provides the use of the catalytic fiber prepared by the method described in the first aspect and the catalytic filter bag described in the second aspect in the low-temperature removal of dioxins, NOx and dust in flue gas.
[0021] Beneficial effects of the present invention
[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate, and aluminum oxide as raw materials, and changes are induced in the material structure and performance through the mechanical force of the ball mill, and the transition metal oxide is loaded on the surface of the carrier titanium dioxide. The main active component Ti-VW-Mo and the rare earth metal auxiliary cerium form a catalyst powder with high dispersion, stable structure and high activity, which can not only decompose dioxins, but also denitrify, wherein the rare earth metal auxiliary cerium greatly improves the catalytic activity. The catalyst preparation method is green and pollution-free, the preparation conditions are mild, the cycle is short, it is easy to synthesize on a large scale, and it has low-temperature catalytic activity and stability.
[0023] The catalyst powder and the organic polymer resin powder are fully mixed and stirred in a controlled ratio, and the stirring speed and the drawing temperature are controlled by adding a lubricant. The prepared catalytic fiber filaments have good mechanical tensile properties and thermal stability. The catalytic filter bag prepared by using the catalytic fiber is
[0024] The catalytic fiber and catalytic filter bag prepared by the method of the present invention have a wide applicable temperature range and a long service life. At about 180°C, the catalytic reaction has a dioxin removal efficiency of 98.72%, a NOx removal efficiency of 99.54%, and a dust filtration efficiency of 99.97%. The catalytic filter bag has stable catalytic performance and a long service life, and has achieved good results in the low-temperature removal of flue gas dioxins, NOx and dust. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The SEM image of the catalytic fiber obtained in Example 1 of the present invention is shown;
[0026] Figure 2 The comparison of tensile properties of catalytic fibers under different ratios of organic polymer resin powder to catalyst of the present invention is shown;
[0027] Figure 3 The comparison of tensile properties of the catalytic fibers under different mixing and stirring times of the present invention is shown;
[0028] Figure 4 The comparison of tensile properties of the catalytic fibers at different stretching temperatures of the present invention is shown;
[0029] Figure 5 The thermal stability analysis of the catalytic fiber of the present invention is shown;
[0030] Figure 6 A graph showing the stability of dioxin and NOx removal efficiency of the catalytic filter bag of the present invention is shown. DETAILED DESCRIPTION
[0031] The following examples are used to demonstrate preferred embodiments of the present invention. It will be appreciated by those skilled in the art that the techniques disclosed in the following examples represent techniques discovered by the inventors that can be used to implement the present invention and therefore can be considered as preferred embodiments of the present invention. However, it will be appreciated by those skilled in the art based on this specification that many modifications may be made to the specific embodiments disclosed herein and still achieve the same or similar results without departing from the spirit or scope of the present invention.
[0032] Numerical ranges in this application are approximate values, so unless otherwise specified, they may include numerical values outside the range. Numerical ranges include all numerical values from the lower limit to the upper limit increased by 1 unit, provided that there is an interval of at least 2 units between any lower value and any higher value. For example, if the recorded component, physical or other properties (such as molecular weight, melt index, etc.) are 100 to 1000, it means that all single values are clearly listed, such as 100, 101, 102, etc., and all sub-ranges, such as 100 to 166, 155 to 170, 198 to 200, etc. For a range comprising a numerical value less than 1 or comprising a fraction greater than 1 (such as 1.1, 1.5, etc.), 1 unit is appropriately regarded as 0.0001, 0.001, 0.01 or 0.1. For a range comprising a single digit less than 10 (such as 1 to 5), 1 unit is usually regarded as 0.1. These are only specific examples of what is intended, and all possible combinations of numerical values between the lowest value and the highest value enumerated are to be considered to be expressly stated in this application.
[0033] In the present invention, unless otherwise specified, all molar concentrations and mass fractions are weight units, and the equipment and raw materials used, except for those specifically limited in the present invention, can be purchased from the market or are commonly used in the art. The methods in the following examples, unless otherwise specified, are conventional methods in the art. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs, and the materials publicly cited herein and those cited by them will be incorporated by reference. Those skilled in the art will be aware of or will understand many equivalent technologies for the specific embodiments of the invention described herein through routine experiments. These equivalents will be included in the claims.
[0034] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.
[0035] In the present invention, the titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate, aluminum oxide and other chemicals are all conventional reagents and can be purchased from conventional biochemical reagent manufacturers.
[0036] The polytetrafluoroethylene resin powder of the present invention has a crystallinity of more than 99%, a molecular weight of 2 million to 10 million, an average particle size of 400 to 800 μm, and is a commercially available product (such as Zhejiang Juhua dispersed fine powder resin).
[0037] The liquid lubricant in the present invention is one of the liquid solvents petroleum ether, kerosene and paraffin.
[0038] Example 1 Catalyst Preparation
[0039] Titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate in a mass ratio of 10:1:0.5:0.5:0.1 were mixed evenly and placed in a ball mill. The diameters of the zirconia balls were 10 mm and 5 mm, the mass ratio of large balls to small balls was 1:1, the mass ratio of the balls in the ball mill was 20:1, the rotation speed was 550 rpm, and the ball milling time was 2 h. The obtained powder was then placed in a muffle furnace with an air atmosphere and a heating rate of 5 °C / min. The mixture was maintained at 450 °C for 1 h and calcined to obtain catalyst-1.
[0040] Comparative Example 1
[0041] Titanium dioxide, ammonium metavanadate and ammonium metatungstate in a mass ratio of 10:1:0.5 were mixed evenly and placed in a ball mill. The diameters of the zirconia balls were 10 mm and 5 mm, the mass ratio of the large balls to the small balls was 1:1, the mass ratio of the balls in the ball mill was 20:1, the rotation speed was 550 rpm, and the ball milling time was 2 h. The obtained powder was then placed in a muffle furnace with an air atmosphere and a heating rate of 5 °C / min. The mixture was maintained at 450 °C for 1 h and calcined to obtain catalyst-2.
[0042] Comparative Example 2
[0043] Titanium dioxide, ammonium metavanadate and ammonium molybdate in a mass ratio of 10:1:0.5 were mixed evenly and placed in a ball mill. The diameters of the zirconia balls were 10 mm and 5 mm, the mass ratio of large balls to small balls was 1:1, the mass ratio of the balls in the ball mill was 20:1, the rotation speed was 550 rpm, and the ball milling time was 2 h. The obtained powder was then placed in a muffle furnace with an air atmosphere and a heating rate of 5 °C / min. The mixture was maintained at 450 °C for 1 h and calcined to obtain catalyst-3.
[0044] Comparative Example 3
[0045] Titanium dioxide, ammonium metavanadate, ammonium metatungstate and ammonium molybdate in a mass ratio of 10:1:0.5:0.5 were mixed evenly and placed in a ball mill. The diameters of the zirconia balls were 10 mm and 5 mm, the mass ratio of large balls to small balls was 1:1, the mass ratio of the balls in the ball mill was 20:1, the rotation speed was 550 rpm, and the ball milling time was 2 h. The obtained powder was then placed in a muffle furnace with an air atmosphere and a heating rate of 5 °C / min. The mixture was maintained at 450 °C for 1 h and calcined to obtain catalyst-4.
[0046] Example 2 SEM Characterization of Catalytic Fibers
[0047] The catalyst-1 prepared in Example 1 was sieved with a 400-mesh sieve, and 27 g of catalyst-1 powder was taken.
[0048] After surface modification, it is evenly mixed with 250g of polytetrafluoroethylene resin powder, and then 50g of liquid lubricant petroleum ether and additive alumina are added and stirred for 30 minutes. The mixture is allowed to stand at room temperature for 120 hours, and then dried at 50°C for 12 hours to fully mix the polytetrafluoroethylene resin powder, catalyst powder and liquid lubricant to form a catalytic material.
[0049] The blank was made on a blanking machine at room temperature, extruded into a rod-shaped product by an extruder, and then calendered into a base tape at 50°C. After that, it was longitudinally stretched at 200°C to form a defatted base tape, sintered at 350°C for 60 seconds to form a sintered base tape, and finally the base tape was opened in a fiber opening device to obtain polytetrafluoroethylene catalytic fiber-1.
[0050] The polytetrafluoroethylene catalytic fiber-1 was observed by SEM. The SEM image of the catalytic fiber is shown in Figure 1 shown.
[0051] The results showed that catalyst particles existed on the surface and inside of the catalytic fibers.
[0052] Example 3 Thermal stability of catalytic fibers
[0053] The polytetrafluoroethylene catalytic fiber-1 prepared in Example 2 was analyzed using a Swiss Mettler synchronous thermal analyzer, instrument model TGA / DSC 3+.
[0054] Comparative analysis of thermal stability between catalytic fiber and blank fiber Figure 2 shown.
[0055] The results show that below 450°C, the fiber structure is stable and the doping of catalyst will not affect the thermal stability of the fiber.
[0056] Example 4: Ratio of catalyst to PTFE and tensile properties of catalytic fibers
[0057] 27g, 62.5g, 107g, and 166g of catalyst-1 were surface modified and evenly mixed with 250g of polytetrafluoroethylene resin powder, and then 50g of liquid lubricant petroleum ether and additive alumina were added and stirred for 30 minutes, and then allowed to stand at room temperature for 120 hours, and then dried at 50°C for 12 hours to fully mix the polytetrafluoroethylene resin powder, catalyst powder, liquid lubricant, and additives to form a catalytic material. A blank was made on a blanking machine at room temperature, a rod was extruded through an extruder, and then calendered into a base tape at 50°C. After that, it was longitudinally stretched at 200°C to form a degreased base tape, sintered at 350°C for 60 seconds to form a sintered base tape, and finally the base tape was opened in a fiber opening device to obtain polytetrafluoroethylene catalytic fiber.
[0058] The relationship between the ratio of different catalysts and PTFE and the elongation at break of catalytic fibers is as follows: Figure 3 shown.
[0059] The results show that as the proportion of catalyst decreases, the tensile properties of the catalytic fiber gradually increase. When the ratio of PTFE to catalyst is 9:1, the elongation at break of the catalytic fiber is about 30%.
[0060] Example 5 Stirring time during preparation and tensile properties of catalytic fibers
[0061] 27g of catalyst-1 surface modified and 250g of polytetrafluoroethylene resin powder were uniformly mixed, and then 50g of liquid lubricant petroleum ether and additive alumina were added, and the mixture was stirred for 5min, 10min, and 30min respectively, and allowed to stand at room temperature for 120h, and then dried at 50℃ for 12h to fully mix the polytetrafluoroethylene resin powder, catalyst powder, liquid lubricant, and additive to form a catalytic material. The blank was made on a blanking machine at room temperature, extruded into a rod-shaped object through an extruder, and then calendered into a base tape at 50℃. After that, it was longitudinally stretched at 200℃ to form a degreased base tape, sintered and fixed at 350℃ for 60 seconds to form a sintered base tape, and finally the base tape was opened in a fiber opening device to obtain polytetrafluoroethylene catalytic fiber.
[0062] The relationship between different stirring times during the preparation process and the breaking elongation of the catalytic fiber is as follows: Figure 4 shown.
[0063] The results showed that as the stirring time increased, the elongation at break of the catalytic fiber also increased. When the stirring time was about 30 minutes, the elongation at break was about 31.
[0064] Example 6 Different stretching temperatures during the preparation process and tensile properties of catalytic fibers
[0065] 27g of catalyst-1 surface modified and 250g of polytetrafluoroethylene resin powder were uniformly mixed, and then 50g of liquid lubricant petroleum ether and additive alumina were added, mixed and stirred for 30 minutes, left to stand at room temperature for 120 hours, and then dried at 50°C for 12 hours to fully mix the polytetrafluoroethylene resin powder, catalyst powder, liquid lubricant and additive to form a catalytic material. The blank was made on a blanking machine at room temperature, extruded into a rod-shaped object through an extruder, and then calendered into a base tape at 50°C. After that, it was longitudinally stretched into a degreased base tape at 100°C, 150°C, 200°C, 250°C, and 300°C, respectively, sintered and shaped at 350°C for 60 seconds to form a sintered base tape, and finally the base tape was opened in a fiber opening device to obtain polytetrafluoroethylene catalytic fiber.
[0066] The relationship between different stretching temperatures during the preparation process and the breaking elongation of the catalytic fiber is as follows: Figure 5 shown.
[0067] The results show that when the stretching temperature is greater than 200°C, the breaking elongation of the catalytic fiber is above 30, and when the stretching temperature is 200°C, the breaking elongation of the catalytic fiber is the best.
[0068] Example 7 Performance test of catalytic filter bag for catalytic degradation of dioxins, NOx and dust removal
[0069] The catalysts-1, -2, -3 and -4 for low-temperature catalytic dioxin prepared in Example 1 and Comparative Examples 1-3 were sieved with a 400-mesh sieve, 27 g of catalyst powder was surface-modified and then evenly mixed with 250 g of polytetrafluoroethylene resin powder, and then 50 g of liquid lubricant petroleum ether and additive alumina were added and stirred for 30 min, and then allowed to stand at room temperature for 120 h, and then dried at 50 ° C for 12 h, so that the polytetrafluoroethylene resin powder, catalyst powder, liquid lubricant and additive were fully mixed to form a catalytic material. A blank was made on a blanking machine at room temperature, a rod was extruded by an extruder, and then calendered into a base tape at 50 ° C. Afterwards, it was longitudinally stretched at 200 ° C to form a defatted base tape, sintered at 350 ° C for 60 seconds to form a sintered base tape, and finally the base tape was opened in a fiber opening device to obtain the corresponding catalytic fiber-1, catalytic fiber-2, catalytic fiber-3, and catalytic fiber-4.
[0070] The catalytic fiber is used as raw material, and the needle-punched felt is obtained through rough opening, cotton mixing box, carding machine, cross-lapping machine, pre-needling and main needling. Then, the catalytic filter bag-1, catalytic filter bag-2, catalytic filter bag-3 and catalytic filter bag-4 are obtained through the processes of impregnation, drying and coating.
[0071] Take a 20mm diameter disc of the catalytic filter bag and place it in the reaction tube. The reaction temperature is 180℃ and the dioxin source concentration is 5.0ngI-TEQ / Nm 3 , nitrogen and oxygen were introduced, the oxygen content was 11%, and the total gas flow rate was 500ml / min, and the dioxin catalytic performance and denitrification performance were tested; the dust filtration efficiency test was carried out in accordance with the standard ISO 11057, using a filter material simulation test device, and the test results are shown in Table 1 and Figure 6 shown.
[0072] Table 1 Removal efficiency of catalytic filter bags for dioxins, NOx and dust
[0073] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Dioxin removal efficiency (%) 98.72 85.6 89.3 91.0 NOx removal efficiency (%) 99.54 84.9 89.5 92.5 Filtration efficiency (%) 99.97 99.9 99.9 99.9
[0074] The results show that the catalytic fibers and catalytic filter bags prepared using titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate as raw materials have significantly better removal efficiency for dioxins, NOx and dust than other solutions under low-temperature catalytic conditions (about 180°C); it can be seen from Example 1 and Comparative Examples 1-3 that the change in the ratio of catalyst raw materials has an important influence on the performance of the catalyst. Under the synergistic effect of suitable active ingredients, additives and carriers, combined with the control of parameters in the preparation process, the catalytic fibers and catalytic filter bags prepared in Example 1 can achieve a dioxin removal efficiency of 98.72%, a NOx removal efficiency of 99.54%, and a dust filtration efficiency of 99.97%.
[0075] Depend on Figure 6 It can be seen that with the extension of the use time, the removal efficiency of the catalytic filter bag prepared in Example 1 for dioxins and NOx does not decrease significantly, and the stability is good. After the catalytic oxidation reaction lasts for 360 minutes, the removal efficiency of the catalytic filter bag for dioxins and NOx is stabilized at 97.21% and 98.35%.
[0076] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as references separately. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined in the present application.
Claims
1. A method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature, characterized in that: The steps include: (1) Preparation of catalyst powder: using titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate as raw materials, and performing doping by ball milling in a ball mill to obtain catalyst powder; (2) Surface modification of catalyst powder: Add the catalyst powder to the highly concentrated PTFE resin emulsion, with the mass ratio of catalyst to PTFE emulsion being 1:(3-6), ultrasonic frequency being 10-30kHz and the oscillation time being 20-40min, and then put into an oven to dry at 60-80℃; (3) Preparing catalytic fibers: uniformly mixing the catalyst powder after surface modification in step (2) with the organic polymer resin powder, adding a lubricant and an additive and mixing for 25-35 minutes, standing at 20-40°C for 72-120 hours, and then standing at 40-80°C for 12-24 hours for maturation; pressing the mixed material into a blank at 20-30°C, and then extruding and calendering it into a base tape at 40-60°C, degreasing and stretching it at 180-300°C to form a degreased base tape, and heat-setting it at 320-420°C for 20-80 seconds to form a sintered base tape, and opening it on a fiber opening device to obtain catalytic fibers; Among the raw materials, the mass ratio of titanium dioxide, ammonium metavanadate, ammonium metatungstate, ammonium molybdate and cerium nitrate is: (8-12): (0.8-1.2): (0.4-0.6): (0.4-0.6): (0.08-0.12); The ball-to-material mass ratio in the ball mill is 5:1-30:1, the rotation speed is 400-800 r / min, the ball milling time is 2-10 hours, and the powder obtained by ball milling is calcined in an air atmosphere at 400-600° C. for 3-6 hours; The mass ratio of the catalyst powder to the organic polymer resin powder is 1:(9-100); The low temperature is 180°C.
2. The method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature according to claim 1, characterized in that: The mass ratio of organic polymer resin powder to lubricant is (4-5):
1.
3. The method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature according to claim 1, characterized in that: The lubricant used is one of the liquid solvent petroleum ether, kerosene, and paraffin; the additive is one of aluminum oxide and aluminum.
4. The method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature according to claim 1, characterized in that: The organic polymer resin powder is one of polytetrafluoroethylene, polyphenylene sulfide and polyimide.
5. The method for preparing a catalytic fiber for removing dioxins, NOx and dust from flue gas at low temperature according to claim 4, characterized in that: The crystallinity of the organic polymer resin powder is above 99%.
6. A catalytic filter bag, characterized in that: The catalytic filter bag is prepared by the catalytic fiber according to any one of claims 1 to 5, and the needle-punched felt is obtained by rough opening, cotton mixing box, fine opening, air pressure cotton box, carding machine, cross-lapping machine, pre-needling, main needling, trimming and winding. The needle-punched felt is obtained by impregnation, drying, coating and sewing.